Anti-sintering hydrogenation catalyst and application thereof in preparation of hexafluoropropane

By using a catalyst composed of metals such as Pd, Cu, Li, K, etc. to support the pretreated activated carbon support in the hexafluoropropylene hydrogenation process, the problem of sintering of Pd/AC catalysts is solved, and the service life and reaction efficiency of the catalyst are improved. A high conversion rate and high selectivity R236ea preparation was achieved.

CN118904355APending Publication Date: 2024-11-08ZHEJIANG XINGTENG CHEM

Patent Information

Application Number
CN202411056209.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing hexafluoropropylene hydrogenation process, Pd/AC catalysts are prone to sintering, resulting in a low service life and are difficult to effectively use in industrial applications.

Method used

A catalyst composed of metals such as Pd, Cu, Li, K is supported on the pretreated activated carbon support, and an anti-sintering hydrogenation catalyst is prepared by pretreatment of acidic and sodium hypochlorite pretreatment, metal source impregnation and hydrogen-nitrogen treatment.

Benefits of technology

The service life of the catalyst was significantly improved, the conversion rate of hexafluoropropylene reached 99.9%, the selectivity of R236ea reached 99.5%, and there was no significant attenuation after catalyst use for more than 2300 hours.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904355A_ABST
    Figure CN118904355A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-sintering hydrogenation catalyst and application thereof in preparation of hexafluoropropane, the hydrogenation catalyst is formed by loading a main catalyst and an auxiliary agent on an activated carbon carrier, the main catalyst is Pd, and the auxiliary agent is any one or a combination of more than two of Cu, Li and K. According to the present invention, the auxiliary agent in the catalyst can form the strong interaction with the main catalyst Pd so as to inhibit the sintering of the Pd species in the reaction system, and the experiment verification results show that the prepared catalyst has the long service life compared with the conventional Pd / AC catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to fluorine chemical technology, and specifically relates to a hexafluoropropylene hydrogenation process. Background Art

[0002] 1,1,1,2,3,3-hexafluoropropane (R236ea) is a hydrofluorocarbon that can be used as a refrigerant, fire extinguisher, cleaning agent, foaming agent, etching agent and heat carrier, etc. In particular, in the synthesis process of the fourth-generation refrigerant 2,3,3,3-tetrafluoropropene, R236ea is one of the important intermediates and has a wide range of applications and industrial utilization value. Therefore, it is of great significance to develop a high-purity, low-cost preparation process.

[0003] Among all the R236ea synthesis methods, only the hexafluoropropylene hydrogenation process has achieved industrial application due to its advantages such as convenient raw material sources, simple process, high raw material utilization rate, and low energy consumption. Supported palladium catalysts are the most important catalysts in the existing hexafluoropropylene hydrogenation process due to their high activity and high selectivity.

[0004] Chinese patent CN102026947A discloses a method for synthesizing 1,1,1,2,3,3-hexafluoropropane by hydrogenation of hexafluoropropylene using 0.5% Pd / AC catalyst. From the data provided in Example 1, it can be seen that in the case of co-feeding of two components 1,2,3,3,3-pentafluoropropylene (Z-1225ye) and hexafluoropropylene, the conversion rate of hexafluoropropylene is still 85.8%, and the selectivity of 1,1,1,2,3,3-hexafluoropropane is still 93.1% at this conversion rate.

[0005] Chinese patent CN101921168B discloses a method for synthesizing R236ea by catalytic hydrogenation of hexafluoropropylene and hydrogen under the catalytic action of a supported palladium catalyst, wherein palladium is an active component and the carrier is α-alumina. At a maximum reaction temperature of 121°C, the hexafluoropropylene conversion rate can reach 100% and the selectivity of R236ea can reach 99.34%.

[0006] Chinese patent CN105107491B discloses a method for manufacturing and application of a hexafluoropropylene hydrogenation catalyst, wherein the catalyst is composed of a main catalyst, an auxiliary agent and a carrier, wherein the main catalyst is palladium, and the auxiliary agent is a lanthanide metal including one or more of La, Ce, and Pr, and the main catalyst and the auxiliary agent are loaded on an activated carbon carrier. The Pd / AC catalyst prepared by the steps of rapid reduction treatment in the preparation method has uniform distribution of metal Pd, high dispersion, small particle size, and excellent reaction performance. In the gas-phase hydrogenation reaction of hexafluoropropylene, the catalyst has a hexafluoropropylene conversion rate greater than 99%, and an R236ea selectivity greater than 99.5%, and has high activity and high selectivity.

[0007] In the prior art, there are several patents that disclose methods for hydrogenating hexafluoropropylene using Pd / AC catalyst as a hydrogenation catalyst, but only disclose data on reaction conversion rate and target product selectivity, and no data on long-term service life is disclosed. In the experiment of using Pd / AC catalyst to hydrogenate hexafluoropropylene to synthesize R236ea, the applicant found that although the catalytic activity and selectivity of Pd / AC catalyst are high, there is a phenomenon of Pd particle sintering during the reaction, resulting in a relatively low service life of Pd / AC catalyst, making it difficult to apply in industrialization. Summary of the invention

[0008] In view of the defects of the prior art, the present invention provides a sintering-resistant hydrogenation catalyst and its application in the preparation of hexafluoropropane, which solves the problems of easy sintering and low service life of the Pd / AC catalyst used in the hydrogenation reaction of hexafluoropropylene.

[0009] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0010] Firstly, a hydrogenation catalyst is provided, which is formed by a main catalyst and an auxiliary agent loaded on an activated carbon carrier, wherein the main catalyst is Pd, and the auxiliary agent is any one of Cu, Li, and K or a combination of two or more thereof.

[0011] Preferably, the amount of Pd is 0.5-2% of the total mass of the catalyst, and the amount of the auxiliary agent is 0.2-10.0% of the total mass of the catalyst.

[0012] Preferably, the specific surface area of ​​the activated carbon carrier is 1200 to 1800 m2 / g, and the activated carbon carrier is pretreated before use; and / or, the activated carbon carrier is prepared using coconut shell as a carbon source.

[0013] Secondly, a method for preparing a hydrogenation catalyst is provided, which is used to prepare the hydrogenation catalyst, comprising the following steps:

[0014] (1) Carrier pretreatment: The activated carbon is pretreated with acid and sodium hypochlorite;

[0015] (2) Metal source impregnation treatment: The metal salt solution of the main catalyst and the auxiliary agent is impregnated step by step or co-impregnated into the pre-treated activated carbon;

[0016] (3) evaporating the suspension after immersion in step (2) at a drying temperature of 60 to 120° C.;

[0017] (4) The sample dried in step (3) is treated with a hydrogen-nitrogen mixed gas, wherein the volume ratio of hydrogen in the hydrogen-nitrogen mixed gas is 5 to 10%, and the treatment temperature is 150 to 250° C., thereby finally obtaining a highly active hydrogenation catalyst.

[0018] Preferably, in the carrier pretreatment step, the activated carbon is refluxed with a 5-10% hydrochloric acid aqueous solution at 60-90° C. for 2-5 hours, washed with deionized water, and then added to an aqueous solution containing 0.5-7% sodium hypochlorite, stirred for 5-10 hours, filtered, washed, and dried to obtain pretreated activated carbon.

[0019] Preferably, the metal salt of the metal salt solution of the main catalyst is one of palladium chloride, palladium nitrate, palladium acetate, tetraamminepalladium acetate and organic palladium.

[0020] Preferably, the metal salt of the metal salt solution of the auxiliary agent is a nitrate or a halide containing the auxiliary agent element.

[0021] In addition, a method for preparing hexafluoropropane is also provided, which uses the catalyst to hydrogenate and prepare 1,1,1,2,3,3-hexafluoropropane, and reacts hexafluoropropylene, hydrogen and the hydrogenation catalyst at 150-300° C. to obtain 1,1,1,2,3,3-hexafluoropropane.

[0022] Preferably, the reaction pressure is controlled to be normal pressure to 0.5 MPa; and the reaction volume space velocity is controlled to be 300 to 5000 h-1.

[0023] Preferably, the volume ratio of hexafluoropropylene to hydrogen is 1:2 to 1:10.

[0024] The present invention adopts the above technical solution and has the following beneficial effects:

[0025] (1) The auxiliary agent in the catalyst of the present invention can form a strong interaction with the main catalyst Pd, inhibiting the sintering of Pd species in the reaction system. Experimental verification shows that the catalyst prepared by the present invention has a longer service life than the conventional Pd / AC catalyst, thereby reducing the cost of use.

[0026] (2) The catalyst prepared by the present invention is used in the gas-phase catalytic hydrogenation of hexafluoropropylene to produce R236ea. Experimental verification shows that the hexafluoropropylene conversion rate can reach 99.9%, while the R236ea selectivity reaches 99.5%. The catalyst is used for more than 2300 hours without obvious attenuation of reaction activity.

[0027] The specific technical solutions and beneficial effects of the present invention will be described in detail in the following specific embodiments in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments:

[0029] Figure 1 This is an activity diagram for evaluating the life of the catalyst prepared in Example 2;

[0030] Figure 2 This is an activity diagram for evaluating the life of the catalyst prepared in Example 4;

[0031] Figure 3 Activity diagram for Pd / AC catalyst life evaluation;

[0032] Figure 4 TEM images of the catalyst before and after the reaction. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0034] The present invention provides a hydrogenation catalyst, which is formed by a main catalyst and an auxiliary agent loaded on an activated carbon carrier, wherein the main catalyst is Pd, and the auxiliary agent is any one of Cu, Li, and K or a combination of two or more thereof.

[0035] The auxiliary agent in the hydrogenation catalyst of the present invention can form a strong interaction with the main catalyst Pd, inhibiting the sintering of Pd species in the reaction system, and experimental verification shows that the catalyst prepared by the present invention has a longer service life than conventional Pd / AC catalysts.

[0036] The amount of Pd is 0.5-2% of the total mass of the catalyst, such as 0.8%, 1%, 2%. The amount of the auxiliary agent is 0.2-10.0% of the total mass of the catalyst, such as 0.5%, 1%, 2%, 5%, 8%. The specific surface area of ​​the activated carbon carrier is 1200-1800m 2 / g, for example 1200 2 / g, 1500 2 / g, 1800 2 / g. The activated carbon carrier is pretreated before use, and the activated carbon carrier is prepared using coconut shell as a carbon source.

[0037] Furthermore, the preparation method of the above-mentioned hydrogenation catalyst comprises the following steps:

[0038] (1) Carrier pretreatment: The activated carbon is pretreated with acid and sodium hypochlorite;

[0039] (2) Metal source impregnation treatment: The metal salt solution of the main catalyst and the auxiliary agent is impregnated step by step or co-impregnated into the pre-treated activated carbon;

[0040] (3) evaporating the suspension after immersion in step (2) at a drying temperature of 60 to 120° C.;

[0041] (4) The sample dried in step (3) is treated with a hydrogen-nitrogen mixed gas, wherein the volume ratio of hydrogen in the hydrogen-nitrogen mixed gas is 5 to 10%, and the treatment temperature is 150 to 250° C., thereby finally obtaining a highly active hydrogenation catalyst.

[0042] Preferably, in the carrier pretreatment step, the activated carbon is treated with a 5-10% hydrochloric acid aqueous solution at 60-90° C. for 2-5 hours, washed with deionized water, and then added to an aqueous solution containing 0.5-7% sodium hypochlorite, stirred for 5-10 hours, filtered, washed, and dried to obtain pretreated activated carbon. The metal salt of the metal salt solution of the main catalyst is one of palladium chloride, palladium nitrate, palladium acetate, tetraammine palladium acetate, and organic palladium. The metal salt of the metal salt solution of the auxiliary agent is a nitrate or halide containing an auxiliary element.

[0043] As a preferred solution, the pH value of the impregnation solution is in the range of 4 to 8. As a further preferred solution, the pH value of the impregnation solution is in the range of 5 to 7.5. Within this pH value range, the binding capacity between the activated carbon carrier and the impregnation component can be improved.

[0044] In addition, the invention also relates to a method for preparing hexafluoropropane, which adopts the catalyst to hydrogenate and prepare 1,1,1,2,3,3-hexafluoropropane, and comprises reacting hexafluoropropylene, hydrogen and the hydrogenation catalyst at 150-300° C. to obtain 1,1,1,2,3,3-hexafluoropropane.

[0045] Preferably, the reaction pressure is controlled to be normal pressure to 0.5 MPa; the reaction volume space velocity is controlled to be 300 to 5000 h -1 The volume ratio of hexafluoropropylene to hydrogen is 1:2 to 1:10.

[0046] The technical solution of the present invention is described below in conjunction with specific embodiments.

[0047] Example 1

[0048] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 5% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0049] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% by mass of palladium was added dropwise, and 5 g of copper chloride solution containing 1% by mass of copper was added dropwise, and stirred and immersed for 6 hours, and evaporated to dryness at 80°C. Then, the solid sample was taken out and placed in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% by volume of hydrogen, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for hexafluoropropylene hydrogenation reaction.

[0050] Example 2

[0051] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 10% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 5% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0052] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% by mass of palladium was added dropwise, and 5 g of copper chloride solution containing 1% by mass of copper was added dropwise, and stirred and immersed for 6 hours, and evaporated to dryness at 80°C. Then, the solid sample was taken out and placed in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% by volume of hydrogen, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for hexafluoropropylene hydrogenation reaction.

[0053] Example 3

[0054] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 5% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0055] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% by mass of palladium was added dropwise, and 10 g of copper chloride solution containing 1% by mass of copper was added dropwise, and stirred and immersed for 6 hours, and evaporated to dryness at 80°C. Then, the solid sample was taken out and dried in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% by volume of hydrogen, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for hexafluoropropylene hydrogenation reaction.

[0056] Example 4

[0057] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 5% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0058] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% by mass of palladium was added dropwise, and 20 g of copper chloride solution containing 1% by mass of copper was added dropwise, and stirred and immersed for 6 hours, and evaporated to dryness at 80°C. Then, the solid sample was taken out and placed in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% by volume of hydrogen, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for hexafluoropropylene hydrogenation reaction.

[0059] Example 5

[0060] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 2% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0061] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% by mass of palladium was added dropwise, and 5 g of lithium chloride solution containing 1% by mass of lithium was added dropwise, and stirred and immersed for 6 hours, and evaporated to dryness at 80°C. Then, the solid sample was taken out and placed in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% by volume of hydrogen, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for the hydrogenation reaction of hexafluoropropylene.

[0062] Example 6

[0063] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 2% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0064] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% by mass of palladium was added dropwise, and 5 g of potassium chloride solution containing 1% by mass of potassium was added dropwise, and stirred and immersed for 6 hours, and evaporated to dryness at 80°C. Then, the solid sample was taken out and placed in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% by volume of hydrogen, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for hexafluoropropylene hydrogenation reaction.

[0065] Example 7

[0066] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 2% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0067] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% by mass of palladium was added dropwise, and 20 g of lithium chloride solution containing 1% by mass of lithium was added dropwise, and stirred and immersed for 6 hours, and evaporated to dryness at 80°C. Then, the solid sample was taken out and placed in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% by volume of hydrogen, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for the hydrogenation reaction of hexafluoropropylene.

[0068] Example 8

[0069] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 2% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0070] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% by mass of palladium was added dropwise, and 20 g of potassium chloride solution containing 1% by mass of potassium was added dropwise, and stirred and immersed for 6 hours, and evaporated to dryness at 80°C. Then, the solid sample was taken out and placed in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% by volume of hydrogen, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for hexafluoropropylene hydrogenation reaction.

[0071] Example 9

[0072] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 5% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0073] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% by mass of palladium was added dropwise, 5 g of copper chloride solution containing 1% by mass of copper was added dropwise, and 5 g of lithium chloride solution containing 1% by mass of lithium was added dropwise, and stirred and immersed for 6 hours, evaporated to dryness at 80°C, and then the solid sample was taken out and placed in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% by volume of hydrogen, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for hexafluoropropylene hydrogenation reaction.

[0074] Example 10

[0075] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 5% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0076] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% by mass of palladium was added dropwise, 5 g of copper chloride solution containing 1% by mass of copper was added dropwise, and 5 g of potassium chloride solution containing 1% by mass of potassium was added dropwise, and stirred and immersed for 6 hours, evaporated to dryness at 80°C, and then the solid sample was taken out and placed in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% by volume of hydrogen, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for hexafluoropropylene hydrogenation reaction.

[0077] Embodiment 11

[0078] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 5% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0079] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% palladium by mass was added dropwise, 10 g of copper chloride solution containing 1% copper by mass was added dropwise, and 5 g of potassium chloride solution containing 1% potassium by mass was added dropwise, and stirred and immersed for 6 hours, evaporated to dryness at 80°C, and then the solid sample was taken out and placed in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% hydrogen by volume, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for hexafluoropropylene hydrogenation reaction.

[0080] Example 12

[0081] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 5% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0082] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% by mass of palladium was added dropwise, 5 g of copper chloride solution containing 1% by mass of copper was added dropwise, and 10 g of potassium chloride solution containing 1% by mass of potassium was added dropwise, and stirred and immersed for 6 hours, evaporated to dryness at 80°C, and then the solid sample was taken out and placed in an oven at 110°C for 4 hours. Finally, it was placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% by volume of hydrogen, and maintained at this temperature for 4 hours to obtain a catalyst that can be used for hexafluoropropylene hydrogenation reaction.

[0083] Embodiment 13

[0084] Catalyst application experiment: Hexafluoropropylene hydrogenation to prepare R236ea reaction was carried out in a fixed bed reactor under normal pressure. The reactor was made of inconel600 alloy with an inner diameter of 12 mm. 4 ml of the catalyst prepared in Examples 1 to 12 was loaded respectively. The raw material space velocity was 300 h -1 , the reaction temperature is 120℃, the raw material ratio is V HFP :V H2 =1:2, after 4 hours of stable reaction, the composition of the reaction gas after water washing was measured, and the conversion rate and selectivity were calculated. The results are shown in Table 1.

[0085] Table 1 The results of the reaction activity of the catalysts of Examples 1 to 12 in the preparation of R236ea by hydrogenation of hexafluoropropylene

[0086] catalyst HFP conversion rate / % R236ea selectivity / % Example 1 99.3 99.1 Example 2 99.5 99.8 Example 3 99.2 99.7 Example 4 99.4 99.9 Example 5 99.7 99.4 Example 6 99.8 99.7 Example 7 99.6 99.1 Example 8 99.6 99.2 Example 9 99.8 99.7 Example 10 99.6 99.3 Embodiment 11 99.8 99.2 Example 12 99.9 99.8

[0087] Embodiment 14

[0088] The catalyst stability test adopts the same reaction device and reaction conditions as the catalysts in test examples 1 to 12, and the catalysts prepared in examples 2 and 4 are loaded. The composition of the reaction gas after washing is measured every few hours, and the conversion rate and selectivity are calculated. The stability test results are shown in FIG. Figure 1 and 2 shown.

[0089] Combining the above embodiments and Figure 3 , Figure 4 The above catalyst was used in the gas-phase catalytic hydrogenation of hexafluoropropylene to produce R236ea. Experimental verification showed that the hexafluoropropylene conversion rate could reach 99.9%, while the R236ea selectivity reached 99.5%. The catalyst was used for more than 2300 hours without obvious attenuation of reaction activity.

[0090] Comparative Example 1

[0091] (1) Activated carbon pretreatment: 20 g of activated carbon was added to 500 ml of 5% hydrochloric acid aqueous solution and immersed and refluxed at 60° C. for 4 hours, and then the liquid was filtered and washed 3 times. The obtained sample was added to 500 ml of 2% sodium hypochlorite aqueous solution and stirred and immersed for 4 hours, filtered and washed with deionized water until neutral, and dried to obtain pretreated activated carbon;

[0092] (2) Preparation of catalyst: 10 g of pretreated activated carbon was added to 100 ml of deionized water and stirred evenly, then 5 g of palladium chloride solution containing 1% palladium by mass was added dropwise, stirred and immersed for 6 hours, evaporated to dryness at 80°C, then the solid sample was taken out and placed in an oven at 110°C for 4 hours, and finally placed in a muffle furnace and heated from room temperature to 250°C at 2°C / min in an atmosphere of a hydrogen-nitrogen mixed gas containing 5% hydrogen by volume, and maintained at this temperature for 4 hours to obtain a Pd / AC catalyst.

[0093] The stability test of using Pd / AC for hydrogenation of hexafluoropropylene to prepare R236ea was carried out. The same reaction device and reaction conditions as those in the catalysts of test examples 1 to 12 were used. The composition of the reaction gas after washing was measured every few hours, and the conversion rate and selectivity were calculated. The stability test results are shown in FIG. Figure 3 shown.

[0094] From the above Table 1, Figure 1 , Figure 2 and Figure 3It can be seen from the activity results of each catalyst in the embodiment and the comparative example that when the catalyst provided by the present invention is used for the hydrogenation of hexafluoropropylene to prepare R236ea, it has a high conversion rate, target product selectivity and catalytic stability. After 2300 hours of reaction, the catalytic activity still has no significant change. Compared with the Pd / AC catalyst, although the Pd / AC catalyst has a high conversion rate and R236ea selectivity for hexafluoropropylene, the catalyst is easily deactivated in the reaction system and has poor stability. The hexafluoropropylene conversion rate has dropped to 50% after less than 1000 hours of reaction.

[0095] The fresh catalyst prepared in Example 2, the catalyst of Example 2 after life evaluation, the fresh catalyst of Comparative Example 1 and the catalyst of Comparative Example 1 after life evaluation were named as Catalysts 1 to 4, and were characterized by TEM. The results were as follows: Figure 4 As shown in (a) to (d), the dark black images in the TEM images are the loaded active component Pd particles. It can be seen that the particle size of the Pd particles loaded on the catalyst prepared in Example 2 of the present invention did not change significantly before and after the life evaluation, while the Pd particles loaded on the Pd / AC catalyst showed obvious sintering and agglomeration after the life evaluation. The auxiliary component added to the catalyst provided by the present invention can produce a synergistic effect with the main catalyst, greatly improving the anti-sintering performance of the active component palladium and greatly improving the service life of the catalyst.

[0096] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that the present invention includes but is not limited to the contents described in the above specific embodiments. Any modification that does not deviate from the functional and structural principles of the present invention will be included in the scope of the claims.

Claims

1. A hydrogenation catalyst, characterized in that The catalyst is formed by loading a main catalyst and an auxiliary agent on an activated carbon carrier, wherein the main catalyst is Pd, and the auxiliary agent is any one of Cu, Li, and K or a combination of two or more thereof.

2. A hydrogenation catalyst according to claim 1, characterized in that: The amount of Pd used is 0.5-2% of the total mass of the catalyst, and the amount of the auxiliary agent used is 0.2-10.0% of the total mass of the catalyst.

3. A hydrogenation catalyst according to claim 1, characterized in that: The specific surface area of ​​the activated carbon carrier is 1200 to 1800 m 2 / g, and the activated carbon carrier is pretreated before use; and / or, the activated carbon carrier is prepared using coconut shell as a carbon source.

4. A method for preparing a hydrogenation catalyst, for preparing the hydrogenation catalyst according to any one of claims 1 to 3, characterized in that: The steps include: (1) Carrier pretreatment: The activated carbon is pretreated with acid and sodium hypochlorite; (2) Metal source impregnation treatment: The metal salt solution of the main catalyst and the auxiliary agent is impregnated step by step or co-impregnated into the pre-treated activated carbon; (3) evaporating the suspension after immersion in step (2) at a drying temperature of 60 to 120° C.; (4) The sample dried in step (3) is treated with a hydrogen-nitrogen mixed gas, wherein the volume ratio of hydrogen in the hydrogen-nitrogen mixed gas is 5 to 10%, and the treatment temperature is 150 to 250° C., thereby finally obtaining a highly active hydrogenation catalyst.

5. The method for preparing a hydrogenation catalyst according to claim 4, characterized in that: In the carrier pretreatment step, the activated carbon is refluxed with a 5-10% hydrochloric acid aqueous solution at 60-90° C. for 2-5 hours, washed with deionized water, and then added to an aqueous solution containing 0.5-7% sodium hypochlorite, stirred for 5-10 hours, filtered, washed, and dried to obtain pretreated activated carbon.

6. The method for preparing a hydrogenation catalyst according to claim 4, characterized in that: The metal salt of the metal salt solution of the main catalyst is one of palladium chloride, palladium nitrate, palladium acetate, tetraamminepalladium acetate and organic palladium.

7. The method for preparing a hydrogenation catalyst according to claim 4, characterized in that: The metal salt of the metal salt solution of the auxiliary agent is a nitrate or a halide containing an auxiliary agent element.

8. A method for preparing hexafluoropropane, comprising preparing 1,1,1,2,3,3-hexafluoropropane by hydrogenation using the catalyst according to any one of claims 1 to 3, characterized in that: Hexafluoropropylene, hydrogen and the hydrogenation catalyst are reacted at 150-300° C. to obtain 1,1,1,2,3,3-hexafluoropropane.

9. The method for preparing hexafluoropropane according to claim 8, characterized in that: The reaction pressure is controlled at atmospheric pressure to 0.5 MPa; the reaction volume space velocity is controlled at 300 to 5000 h -1 .

10. The method for preparing hexafluoropropane according to claim 8, characterized in that: The volume ratio of hexafluoropropylene to hydrogen is 1:2 to 1:10.

Citation Information

Patent Citations

  • Method for preparing 1,1,1,2,3,3-hexafluoropropane from 1,1,1,2,3,3-hexafluoropropylene and hydrogen gas

    CN101148395A

  • Carbon loaded type noble metal catalyst and preparation method thereof

    CN101450308A

  • Process for the preparation of 2, 3, 3, 3-trifluoropropene

    CN102026947A

  • Synthesis of 2,3,3,3-tetrafluoropropylene

    CN102267869A

  • Catalysts, preparation methods, and applications of gas-phase catalytic hydrogenation of hexafluoroacetone hydrate to hexafluoroisopropanol.