Sea urchin-shaped Nb2C MXene / W18O49 photo-thermal material as well as preparation method and application thereof

Through the preparation of sea urchin-like Nb2C MXene/W18O49 photothermal materials, the heterojunction structure of Nb2C MXene and W18O49 is used to solve the problems of low CO2 reduction yield and poor selectivity in the prior art, and efficient photothermal catalytic reduction is achieved CO2, the selectivity of CO2 conversion to methane reaches more than 75%.

CN118904372AActive Publication Date: 2024-11-08SHAANXI UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410916273.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-08
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The problems of low CO2 reduction yield and poor selectivity in the prior art lead to the inability to obtain higher photocatalytic properties.

Method used

By preparing sea urchin-shaped Nb2C MXene/W18O49 photothermal material, heterojunctions were formed by ultrasonic dispersion and ultraviolet light irradiation. Nb2C MXene was assembled as "flower core" and nanowire-shaped W18O49 was assembled as "petal", forming sea urchin structures and strengthening Photothermal catalytic activity.

Benefits of technology

The activity and selectivity of photothermal catalytic reduction of CO2 are improved. The selectivity of CO2 conversion to methane reaches more than 75%, and the process is simple and does not require a high temperature and high pressure environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004935185130000011
    Figure HDA0004935185130000011
  • Figure HDA0004935185130000012
    Figure HDA0004935185130000012
  • Figure HDA0004935185130000021
    Figure HDA0004935185130000021
Patent Text Reader

Abstract

The invention provides a sea urchin-shaped Nb2C MXene / W18O49 photo-thermal material as well as a preparation method and application thereof. The preparation method comprises the following steps: step 1, dispersing Nb2C MXene powder into ethanol, and carrying out ultrasonic treatment to obtain a turbid liquid A; step 2, dispersing W18O49 into ethanol, and carrying out ultrasonic treatment to obtain a turbid liquid B; and step 3, respectively carrying out ultraviolet irradiation on the obtained turbid liquid A and turbid liquid B under stirring, then adding the turbid liquid A into the turbid liquid B, carrying out ultraviolet irradiation on the obtained mixed turbid liquid, and washing and drying the obtained solid product to obtain the sea urchin-shaped Nb2C MXene / W18O49 heterojunction photocatalyst. The LSPR effect of storing electrons and holes of the sea urchin-shaped Nb2CMXene / W18O49 heterojunction and the sea urchin-shaped rapid CO2 adsorption capability synergistically enhance the reduction activity and selectivity of hydrogen production of methane through photo-thermal catalytic reduction of CO2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of composite materials for environmental protection and solar energy utilization, and is specifically a sea urchin-shaped Nb2CMXene / W 18 O 49 Photothermal material and its preparation method and application. Background Art

[0002] With the acceleration of industrialization, the sharp increase in global carbon dioxide concentration has caused a very serious greenhouse effect. Therefore, reducing the concentration of carbon dioxide in the atmosphere to mitigate the greenhouse effect has become one of the main issues that need to be addressed. In order to reduce the concentration of carbon dioxide in the atmosphere and realize resource utilization, carbon dioxide is converted into fuel and high-value-added chemical raw materials, which can inhibit the greenhouse effect and alleviate the energy crisis. Under visible light and near-infrared light irradiation, pure phase non-stoichiometric tungsten oxide (W 18 O 49 ) The presence of surface oxygen vacancies leads to plasmon-driven activity. The localized surface plasmon resonance (LSPR) effect can enhance the plasmon W 18 O 49 In the photocatalytic activity in the full spectrum region, oxygen vacancies can also serve as reaction sites to improve the reaction process, so W 18 O 49 can be used as photocatalysts for CO2 conversion. However, due to the low free charge density, these W 18 O 49 The LSPR absorption of nanoparticles is usually located in the near-infrared region, resulting in low CO2 reduction yield and poor selectivity, and unable to achieve higher photocatalytic performance. Summary of the invention

[0003] In view of the problems of low CO2 reduction yield and poor selectivity in the prior art, the present invention provides a sea urchin-shaped Nb2CMXene / W 18 O 49 Photothermal material and its preparation method and application.

[0004] The present invention is achieved through the following technical solutions:

[0005] The present invention provides a sea urchin-shaped Nb2C MXene / W 18 O 49 The method for preparing a photothermal material comprises the following steps:

[0006] Step 1, dispersing Nb2C MXene powder in ethanol and ultrasonicating to obtain suspension A;

[0007] Step 2: W 18 O 49 Disperse in ethanol and sonicate to obtain suspension B;

[0008] Step 3, the obtained suspension A and suspension B are irradiated with ultraviolet light respectively under stirring, and then the suspension A is added to the suspension B, and the obtained mixed suspension is irradiated with ultraviolet light. The obtained solid product is washed and dried to obtain sea urchin-like Nb2C MXene / W 18 O 49 Heterojunction photocatalysts.

[0009] Preferably, in step 1, the preparation method of the Nb2C MXene powder is: adding Nb2AlC precursor powder to HF solution, and then stirring the obtained mixture solution in a water bath to react, and after the reaction is completed, washing and drying the obtained product to obtain Nb2C MXene.

[0010] Preferably, in step 2, the W 18 O 49 The preparation method is as follows: WCl6 is dissolved in ethanol to obtain a reaction precursor solution, and then the reaction precursor solution is subjected to a hydrothermal reaction, and the obtained precipitate is washed and dried to obtain W 18 O 49 .

[0011] Preferably, in step 3, the obtained suspension A and suspension B are irradiated with ultraviolet light for 30-60 min respectively under stirring.

[0012] Preferably, in step 3, the obtained mixed suspension is irradiated with ultraviolet light for 1-5 hours.

[0013] Preferably, Nb2C MXene and W 18 O 49 The molar ratio is 1:(0.1-0.75).

[0014] The present invention provides a sea urchin-shaped Nb2C MXene / W prepared by the above-mentioned preparation method. 18 O 49 Photothermal materials.

[0015] Preferably, the sea urchin-like Nb2C MXene / W 18 O 49 W in photothermal materials 18 O 49 The morphology is nanowire, W 18 O 49 Distributed on the surface and inside of Nb2C MXene.

[0016] The present invention provides the sea urchin-like Nb2C MXene / W as described above 18 O 49 Application of photothermal materials in photothermal catalytic reduction of CO2 to produce methane.

[0017] Preferably, the sea urchin-like Nb2C MXene / W 18 O 49 The selectivity of the photothermal material for the product methane is above 75%.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention prepares Nb2C MXene as the "flower core" through self-assembly by ultraviolet irradiation, and nanowire-shaped W 18 O 49 Nb2C MXene / W with "sea urchin" structure showing nanowire-like "petals" 18 O 49 Heterojunction. Compared with the MXene / W prepared by in situ hydrothermal 18 O 49 The present invention will not destroy the layered structure of MXene, nor will it consume the energy stored in MXene and W. 18 O 49 The electron hole concentration in the present invention is that the obtained Nb2CMXene suspension and W 18 O 49 The suspension was irradiated with UV light under stirring to make Nb2CMXene and W 18 O 49 Positive and negative charges are distributed at both ends of the surface, and the electrostatic attraction W 18 O 49 The negatively charged end of the surface and the positively charged end of the Nb2CMXene surface self-assemble to form the "sea urchin" structure Nb2CMXene / W 18 O 49 The preparation process of the present invention is simple and does not require a high temperature and high pressure environment.

[0020] Nb2C MXene / W prepared by the present invention 18 O 49 Heterojunction, due to W 18 O 49 There is W in the structure 5+ / W 6+ , Nb2C MXene contains Nb 5+ , Nb 4+ and Nb 3+ ,Nb2C MXene / W 18 O 49 A large number of electrons and holes are stored in the heterojunction. When used for photothermal catalytic reduction of CO2, high-energy hot holes are formed through the LSPR effect of holes distributed on the surface of Nb2CMXene crystals in the photothermal material to dissociate H2 into H + , dissociated H + The nanowire W18 O 49 CO2 adsorbed by the "petals" is reduced to form H2O, and Nb2C MXene and W 18 O 49 The effect of the interfacial Schottky junction transforms the LSPR effect of Nb2C MXene into high-energy electrons and W 18 O 49 The photoexcitation-generated electrons replenish the nanowire-shaped W 18 O 49 The LSPR effect continuously generates high-energy hot electrons, converting the CO2 adsorbed on the sea urchin-like surface into *CO2 - , b-HCO3, HCOO, HCOO further releases ·OH and cyclically reduces to form CH4. Sea urchin-like Nb2CMXene / W 18 O 49 The LSPR effect of heterojunction storage of electrons and holes and the urchin-like ability to rapidly adsorb CO2 synergistically enhance the reduction activity and selectivity of photothermal catalytic reduction of CO2 to hydrogenate methanogenesis. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 The XRD pattern of the photothermal material prepared in the present invention;

[0023] Figure 2 This is the SEM of the comparative example 1Nb2C MXene of the present invention;

[0024] Figure 3 Comparative Example 2W of the present invention 18 O 49 SEM images of

[0025] Figure 4 Nb2C MXene / W prepared in Example 3 of the present invention 18 O 49 TEM images of

[0026] Figure 5 Nb2C MXene / W prepared in Example 3 of the present invention 18 O 49 HRTEM images of

[0027] Figure 6The UV-Vis-NIR DRS spectrum of the photothermal material prepared in the present invention;

[0028] Figure 7 Nb2C MXene / W prepared in Example 3 of the present invention 18 O 49 MB absorbance curve under dark conditions;

[0029] Figure 8 Nb2C MXene / W prepared in Example 3 of the present invention 18 O 49 EPR spectrum of holes under dark conditions;

[0030] Fig. 9 This is a graph showing the CO2 conversion rate of the photothermal material prepared in the present invention;

[0031] Fig.10 The CH4 selectivity diagram of the photothermal material prepared in the present invention;

[0032] Fig.11 The photothermal reduction CO2 conversion rate at different times in Comparative Example 2 and Example 3 of the present invention;

[0033] Fig.12 Nb2C MXene / W prepared in Example 3 of the present invention 18 O 49 Photothermal reduction of CO2 cycle diagram;

[0034] Fig.13 Nb2C MXene / W prepared in Example 3 of the present invention 18 O 49 The CO and CH4 yield graphs were detected in the experiments without heat source, without light source, without heat source and light source, and with N2 replacing CO2;

[0035] Fig.14 Nb2C MXene / W prepared in Example 3 of the present invention 18 O 49 The change of surface temperature tested by infrared thermal imager. DETAILED DESCRIPTION

[0036] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0037] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.

[0038] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.

[0039] Comparative Example 1

[0040] Step 1: Slowly add Nb2AlC powder at a ratio of 0.05 g / mL into 40 mL HF solution within 10 min to form a mixed solution.

[0041] Step 2: The mixed solution was stirred continuously at 600 r / min for 96 h in a water bath temperature of 55°C.

[0042] Step 3: The mixed solution stirred for 96 h was transferred to a centrifuge tube, and the obtained product was washed with deionized water until the pH of the supernatant reached about 6 to 7. The obtained product was vacuum dried at 60 ° C for 12 h to obtain Nb2CMXene.

[0043] Comparative Example 2

[0044] Step 1: Dissolve 1 mmol of WCl6 in 30 ml of ethanol and stir magnetically for 30 min to obtain a reaction precursor solution.

[0045] Step 2: Transfer the reaction precursor solution to a 50 ml hydrothermal kettle, perform hydrothermal reaction at 180°C for 24 hours, and then cool to room temperature to obtain a precipitate.

[0046] Step 1: The obtained precipitate was washed with deionized water and anhydrous ethanol three times respectively, and dried at 70°C for 12 h to obtain W 18 O 49 .

[0047] Embodiment 1:

[0048] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0049] Step 2, 0.10 mmol W 18 O 49Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0050] Step 3: The obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 30 min under continuous magnetic stirring. Suspension B was slowly added to suspension A, and the mixed suspension was irradiated under ultraviolet light for 3 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W. 18 O 49 Heterojunction photocatalysts.

[0051] Embodiment 2:

[0052] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0053] Step 2, 0.20 mmol W 18 O 49 Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0054] Step 3: The obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 30 min under continuous magnetic stirring. Suspension B was slowly added to suspension A, and the mixed suspension was irradiated under ultraviolet light for 3 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W. 18 O 49 Heterojunction photocatalysts.

[0055] Embodiment 3:

[0056] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0057] Step 2, 0.50 mmol W 18 O 49 Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0058] Step 3: The obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 30 min under continuous magnetic stirring. Suspension B was slowly added to suspension A, and the mixed suspension was irradiated under ultraviolet light for 3 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W. 18 O 49Heterojunction photocatalysts.

[0059] Embodiment 4:

[0060] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0061] Step 2, 0.75 mmol W 18 O 49 Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0062] Step 3: The obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 30 min under continuous magnetic stirring. Suspension B was slowly added to suspension A, and the mixed suspension was irradiated under ultraviolet light for 3 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W. 18 O 49 Heterojunction photocatalysts.

[0063] Embodiment 5:

[0064] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0065] Step 2, 0.50 mmol W 18 O 49 Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0066] Step 3: The obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 30 min under continuous magnetic stirring. The suspension B was slowly added to the suspension A, and the mixed suspension was irradiated under ultraviolet light for 1 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W. 18 O 49 Heterojunction photocatalysts.

[0067] Embodiment 6:

[0068] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0069] Step 2, 0.50 mmol W 18 O 49Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0070] Step 3: The obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 30 min under continuous magnetic stirring. Suspension B was slowly added to suspension A, and the mixed suspension was irradiated under ultraviolet light for 2 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W. 18 O 49 Heterojunction photocatalysts.

[0071] Embodiment 7:

[0072] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0073] Step 2, 0.50 mmol W 18 O 49 Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0074] Step 3: The obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 30 min under continuous magnetic stirring. Suspension B was slowly added to suspension A, and the mixed suspension was irradiated under ultraviolet light for 4 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W. 18 O 49 Heterojunction photocatalysts.

[0075] Embodiment 8:

[0076] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0077] Step 2, 0.50 mmol W 18 O 49 Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0078] Step 3: The obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 30 min under continuous magnetic stirring. Suspension B was slowly added to suspension A, and the mixed suspension was irradiated under ultraviolet light for 4 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W. 18 O 49Heterojunction photocatalysts.

[0079] Embodiment 9:

[0080] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0081] Step 2, 0.50 mmol W 18 O 49 Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0082] Step 3: The obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 30 min under continuous magnetic stirring. Suspension B was slowly added to suspension A, and the mixed suspension was irradiated under ultraviolet light for 5 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W. 18 O 49 Heterojunction photocatalysts.

[0083] Embodiment 10:

[0084] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0085] Step 2, 0.50 mmol W 18 O 49 Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0086] Step 3, the obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 40 min under continuous magnetic stirring. Suspension B was slowly added to suspension A, and the mixed suspension was irradiated under ultraviolet light for 3 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W 18 O 49 Heterojunction photocatalysts.

[0087] Embodiment 11:

[0088] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0089] Step 2, 0.50 mmol W 18 O 49Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0090] Step 3, the obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 50 min under continuous magnetic stirring. Suspension B was slowly added to suspension A, and the mixed suspension was irradiated under ultraviolet light for 3 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W 18 O 49 Heterojunction photocatalysts.

[0091] Embodiment 12:

[0092] Step 1: Disperse 1 mmol of Nb2C MXene powder in 20 ml of ethanol and ultrasonically treat for 30 min to obtain a uniform suspension A.

[0093] Step 2, 0.50 mmol W 18 O 49 Disperse into 20 ml of ethanol and treat by ultrasound for 30 min to obtain a uniform suspension B.

[0094] Step 3, the obtained suspensions A and B were placed in an XPA-3 photochemical reactor, respectively, and irradiated with ultraviolet light for 60 min under continuous magnetic stirring, and the suspension B was slowly added to the suspension A, and the mixed suspension was irradiated under ultraviolet light for 3 h. The obtained powder was washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried at 70 ° C for 12 h to obtain sea urchin-like Nb2C MXene / W 18 O 49 Heterojunction photocatalysts.

[0095] Photothermal CO2 hydrogenation test:

[0096] The existing homemade glass cup was inverted, and the concave part with a diameter of 40 mm at the upper end was regarded as a culture dish. 60 mg of the sea urchin-shaped Nb2C MXene / W of the present invention was taken. 18 O 49 The heterojunction photocatalyst is placed in the culture dish, stirred and dispersed with a small amount of deionized water, and then placed in a vacuum oven, dried under a vacuum environment of 65°C, and taken out for use. While ensuring that the normal-pressure photothermal catalytic device is leak-proof, the normal-pressure photothermal catalytic device is heated to 250°C, the culture dish is placed in the normal-pressure photothermal catalytic device, and an inert gas is continuously passed through the device for 10 minutes (the flow rate is 2mL / min). Close the inlet and outlet valves, and fill the normal-pressure photothermal catalytic device with 20mL of carbon dioxide gas and 60mL of hydrogen. The pressure after inflation is 0.12MPa. React for 3 hours, and take a sample (1mL) into the gas chromatograph every hour to detect the carbon monoxide and methane content. Among them, the light source uses a 300W xenon lamp, and the auxiliary heat temperature is 250°C.

[0097] The accompanying drawings in the present invention are described in detail below.

[0098] Figure 1 Nb2C MXene / W 18 O 49 XRD diagram of heterojunction. For the Nb2C MXene nanosheets in comparative example 1, three clear characteristic diffraction peaks can be found at 9.8°, 33.4°, and 59.4°, which are attributed to the layered stacking structure of Nb2C MXene. 18 O 49 The XRD spectrum of W shows obvious diffraction peaks at 23.2° and 47.5°, corresponding to the monoclinic phase. 18 O 49 (PDF No.84-1516) (010) and (020) planes. Prepared Nb2C MXene / W 18 O 49 The XRD spectra of samples (Example 1, Example 2, Example 3 and Example 4) have both Nb2C MXene and W 18 O 49 The characteristic peaks of Nb2CMXene and W 18 O 49 In addition, it can be observed that Nb2C MXene / W 18 O 49 The characteristic peak of the sample at 9.8° is significantly enhanced compared with that of Nb2C MXene nanosheets, which is presumably due to the partial W 18 O 49 It grows between Nb2C MXene layers, which increases the interlayer spacing.

[0099] exist Figure 2 In the SEM image of Nb2C MXene in Comparative Example 1, a clear layered structure with uniform thickness and interlayer spacing was observed. Figure 3 Comparative Example 2W 18 O 49 In the SEM image, the unique nano-flower ball structure can be clearly observed. These nano-flower ball structures are assembled from nanowires with a length of 1-2 μm. Figure 4 In the TEM image of Example 3, after UV irradiation, W 18 O 49 It appears as dispersed nanowires, and W is grown on the surface and inside of Nb2C MXene. 18 O 49 Nanowires form a "sea urchin" structure, with Nb2C MXene as the "flower core" and W 18 O 49Self-assembled on the surface of Nb2C MXene, presenting nanowire-like "petals". Figure 5 In the HRTEM image of Example 3, the interplanar spacing is 0.38 nm, corresponding to W 18 O 49 (010) crystal plane. This proves the formation of Nb2CMXene / W 18 O 49 Heterojunction.

[0100] Figure 6 Nb2C MXene / W 18 O 49 Heterojunction UV-vis-NIR DRS diagram, all samples of Comparative Examples 1 and 2 and Examples 1 to 4 have light absorption in the UV-visible-near infrared spectrum range of 200 to 2200 nm. The LSPR effect of oxygen vacancies leads to W 18 O 49 The light absorption is significantly enhanced in the entire UV-visible-near infrared range. The heterojunctions of Examples 1 to 4 show obvious absorption shoulders near the light absorption edge due to the presence of oxygen vacancies. Compared with Comparative Example 2, the weakening of the light absorption of the heterojunctions of Examples 1 to 4 is attributed to the interface passivation effect.

[0101] The degradation of Nb2CMXene / W in Example 3 was characterized by using methylene blue MB (70 mg / L) under dark conditions. 18 O 49 The electron concentration stored in the heterojunction itself ( Figure 7 ). This indicates that the electron concentration stored in Example 3 is 432 μmol·g -1 The hole concentration stored in Example 3 was estimated to be 119 μmol·g by EPR quantum spin number test under dark conditions. -1 ( Figure 8 ). In the figure, TEMPO is the quantum spin number L0 of the original single component of 2,2,6,6-tetramethylpiperidinyl oxide under dark conditions. 10min / 20min are TEMPO-MXene / W obtained by electron paramagnetic resonance spectrometer respectively. 18 O 49 The quantum spin number L of the catalyst system after 10 min and 20 min in dark conditions was calculated to obtain the Nb2C MXene / W obtained in step 1. 18 O 49 The hole concentration generated after 20 min in dark conditions was 119 μmol·g -1 This shows that Nb2C MXene / W 18 O 49 The heterogeneous crystal itself stores holes.

[0102] Fig. 9 Nb2C MXene / W 18 O 49 Heterojunction photothermal catalytic reduction of CO2 conversion rate diagram. Under simulated sunlight, due to the W in the structure of comparative example 2, 5+ / W 6+ , so that there are free electrons. After light exposure, the surface plasmon effect (LSPR) occurs, which excites the generation of hot electrons to participate in the reduction reaction of CO2, and the CH4 yield reaches 122μmol·g -1 ·h -1 The CH4 yield of Example 3 reached 184.7 μmol·g -1 ·h -1 For Comparative Example 1, the photothermal catalytic reduction product of CO2 is only CO, while the selectivity of the CO2 reduction product of Comparative Example 2 to CH4 can reach 84.3%. After UV irradiation and recombination, the selectivity of the CO2 reduction product of Example 3 to CH4 reaches 92%, indicating that the CO yield of the composite heterojunction reduction product of CO2 is reduced, and the CH4 yield is increased ( Fig.10 ).

[0103] Fig.11 The photothermal catalytic reduction activity of CO2 in Comparative Example 2 and Example 3 at different time periods is shown. After 5 h of reduction, the yield of CH4 is 218.1 μmol·g -1 ·h -1 、269.2μmol·g -1 ·h -1 . Fig.12 After 6 cycles of testing, the photothermal catalytic reduction CO2 conversion rate in Example 3 is still 180.2 μmol·g -1 ·h -1 , proving that the sample prepared in Example 3 has good cycle stability.

[0104] like Fig.13 As shown, Example 3 Nb2C MXene / W 18 O 49 The total yields of CO and CH4 were 49.3 μmol·g under control conditions (no heating (under xenon light illumination for 3 h), dark (250 °C in dark), and dark without heating (room temperature in dark)). -1 ·h -1 、33.5μmol·g -1 ·h -1 , 9.6 μmol·g -1 ·h -1 , confirming that Nb2C MXene / W 18 O 49The electrons and holes stored in the nanostructured carbon can directly participate in the photothermal catalytic reduction of CO2. Fig.14 In order to use an infrared thermal imager to analyze the Nb2C MXene / W 18 O 49 The surface temperature of the Nb2C MXene / W in Example 3 was tested after 15 minutes of simulated sunlight irradiation. 18 O 49 The surface temperature increased from 29.3℃ to 208℃, indicating that the prepared Nb2C MXene / W 18 O 49 Heterogeneous crystals have good photothermal conversion performance.

Claims

1. A sea urchin-like Nb2C MXene / W 18 O 49 The method for preparing a photothermal material is characterized in that: The steps include: Step 1, dispersing Nb2C MXene powder in ethanol and ultrasonicating to obtain suspension A; Step 2: W 18 O 49 Disperse in ethanol and sonicate to obtain suspension B; Step 3, the obtained suspension A and suspension B are irradiated with ultraviolet light respectively under stirring, and then the suspension A is added to the suspension B, and the obtained mixed suspension is irradiated with ultraviolet light. The obtained solid product is washed and dried to obtain sea urchin-like Nb2C MXene / W 18 O 49 Heterojunction photocatalysts.

2. The sea urchin-shaped Nb2C MXene / W according to claim 1 18 O 49 The method for preparing a photothermal material is characterized in that: In step 1, the preparation method of the Nb2C MXene powder is: adding Nb2AlC precursor powder to HF solution, and then stirring the obtained mixture solution in a water bath to react, and after the reaction is completed, washing and drying the obtained product to obtain Nb2C MXene.

3. The sea urchin-shaped Nb2C MXene / W according to claim 1 18 O 49 The method for preparing a photothermal material is characterized in that: In step 2, the W 18 O 49 The preparation method is as follows: WCl6 is dissolved in ethanol to obtain a reaction precursor solution, and then the reaction precursor solution is subjected to a hydrothermal reaction, and the obtained precipitate is washed and dried to obtain W 18 O 49 .

4. The sea urchin-shaped Nb2C MXene / W according to claim 1 18 O 49 The method for preparing a photothermal material is characterized in that: In step 3, the obtained suspension A and suspension B are irradiated with ultraviolet light for 30-60 minutes respectively under stirring.

5. The sea urchin-shaped Nb2C MXene / W according to claim 1 18 O 49 The method for preparing a photothermal material is characterized in that: In step 3, the obtained mixed suspension is irradiated with ultraviolet light for 1-5 hours.

6. The sea urchin-shaped Nb2C MXene / W according to claim 1 18 O 49 The method for preparing a photothermal material is characterized in that: Nb2C MXene and W 18 O 49 The molar ratio is 1:(0.1-0.75).

7. The sea urchin-like Nb2CMXene / W obtained by the preparation method according to any one of claims 1 to 6 18 O 49 Photothermal materials.

8. The sea urchin-shaped Nb2C MXene / W according to claim 7 18 O 49 The photothermal material is characterized by: The urchin-like Nb2C MXene / W 18 O 49 W in photothermal materials 18 O 49 The morphology is nanowire, W 18 O 49 Distributed on the surface and inside of Nb2C MXene.

9. The sea urchin-like Nb2C MXene / W according to claim 7 18 O 49 Application of photothermal materials in photothermal catalytic reduction of CO2 to produce methane.

10. The use according to claim 9, characterized in that: The urchin-like Nb2CMXene / W 18 O 49 The selectivity of the photothermal material for the product methane is above 75%.

Citation Information

Patent Citations

  • Composite photocatalyst material with sea urchin sphere morphology and preparation method and application thereof

    CN115301262A

  • Preparation method and application of tungsten oxide nanowire / titanium carbide nanosheet composite material

    CN116130256A

  • Energy storage Nb2AlC / Nb2C MXene heterojunction photocatalyst as well as preparation method and application thereof

    CN116943696A

  • Ti2CTx / W18O49 heterojunction-based photoelectrochemical photoelectric detector and preparation method and application thereof

    CN117169303A