6061 aluminum alloy bar extrusion process for automobile probe shell

By optimizing the alloy composition and online solid solution extrusion process, the problems of chromatic defects such as crystal spots and tissue lines after anodization of the 6061 aluminum alloy material were solved, and a small recrystallized structure was formed, which improved the mechanical properties and surface quality.

CN118904959APending Publication Date: 2024-11-08FOSHAN SHENDAMEI SPECIAL ALUMINUM ALLOY CO LTD

Patent Information

Application Number
CN202410962977.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing 6061 aluminum alloy materials often have chromatic defects such as crystal spots and tissue lines after anodization, which affects the surface quality.

Method used

Optimized alloy composition (Si: 0.5-0.7%, Cu: 0.2-0.3%, Mg: 0.9-1.0%, Mn<0.05%, Cr: 0.04-0.07%) and an online water-cooled solution extrusion process, combined with suitable The extrusion rod is gentle at a speed to form a small recrystallization structure, which reduces the recrystallization temperature and prevents secondary recrystallization.

Benefits of technology

Through low manganese, low chromium and large extrusion ratio processes, a large number of dislocations and sub-crystalline structures are formed, the mechanical properties of the material are improved, the crystal spots and line patterns are avoided, and the surface quality is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904959A_ABST
    Figure CN118904959A_ABST
Patent Text Reader

Abstract

The invention provides an extrusion process of a 6061 aluminum alloy bar for an automobile probe shell, and relates to the technical field of aluminum alloy processing, which comprises the following steps: (1) the 6061 aluminum alloy bar comprises the following alloy components: 0.5-0.7% of Si, 0.2-0.3% of Cu, 0.9-1.0% of Mg and Mnlt; 0.05%, and 0.04 to 0.07% of Cr; other components are added according to national standards; (2) a 6061 aluminum alloy bar is taken and heated; (3) extruding on a machine, wherein the extrusion ratio is greater than or equal to 45, the temperature of an extruded cast rod is 490-515 DEG C, and the extrusion speed is greater than or equal to 5mm / s; and (4) on-line water-cooling solid solution treatment. The method has the beneficial effects that the recrystallization temperature is reduced through low manganese, low chromium and large extrusion ratio by optimizing alloy components, low manganese and low chromium and combining reasonable setting and matching of an on-line solid solution extrusion process, proper extrusion rod temperature, extrusion ratio and extrusion speed, and meanwhile, a large number of dislocation and subgrain structures are formed in the extrusion process; a fine recrystallization structure is formed, and meanwhile, secondary recrystallization is prevented. And due to multiple fine recrystallization structure interfaces, the deformation resistance is large, the fine grain strengthening effect is achieved, and the mechanical property is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy processing, in particular to an extrusion process of a 6061 aluminum alloy bar for an automobile probe housing. Background Art

[0002] As the trend of lightweight automobiles becomes increasingly obvious, various lightweight materials are gradually applied to new energy vehicles. Due to the outstanding advantages of aluminum alloy materials in properties and functions, it has become the preferred material for lightweight automobiles. Aluminum alloy is composed of a variety of alloy elements added to the basic element aluminum, and copper, silicon, magnesium, etc. are among them. As the most widely used metal material in industry, it has low density, but relatively high strength and good plasticity. In automotive applications, it has excellent advantages such as light weight, beautiful appearance, impact adsorption, and good weight reduction effect. With the development of intelligent driving, the use of a large number of various probes in new energy vehicles has shown a mainstream trend of using 6061 aluminum alloy materials, but there are extremely high requirements for the surface quality of 6061 aluminum alloy materials after anodizing, and the 6061 materials produced by conventional methods have fibrous crystal structures or coarse recrystallized structures. After anodizing, the appearance of the material often has color defects such as crystal spots and tissue lines.

[0003] Based on this, it is necessary to disclose a 6061 aluminum alloy bar extrusion process for automobile probe housing to overcome the above defects. Summary of the invention

[0004] The present invention overcomes the shortcomings of the prior art and provides a 6061 aluminum alloy bar extrusion process for an automobile probe housing to solve the problem that after anodizing of the 6061 material, the material has color defects such as crystal spots and tissue lines on the surface.

[0005] In order to solve the above technical problems, the present invention is achieved through the following technical solutions:

[0006] A 6061 aluminum alloy bar extrusion process for an automobile probe housing comprises the following steps:

[0007] (1) The cast rod includes the following alloy components: Si: 0.5-0.7%, Cu: 0.2-0.3%, Mg: 0.9-1.0%, Mn<0.05%, Cr: 0.04-0.07%; other additions are in accordance with national standards;

[0008] (2) Take 6061 aluminum alloy bar and heat it;

[0009] (3) Extrusion on the machine, extrusion ratio ≥ 45, extrusion casting temperature 490-515℃, extrusion speed ≥ 5mm / s;

[0010] (4) Online water cooling and solid solution,

[0011] The 6061 aluminum alloy rod is prepared by heating and melting the raw materials, alloying, refining, slagging, standing, degassing and filtering, semi-continuous water-cooling casting, homogenizing and water-cooling.

[0012] Furthermore, the extrusion speed refers to the forward speed of the main cylinder of the extruder.

[0013] Furthermore, after the online water cooling and solution treatment, the aging temperature is 160-175°C and the temperature is kept at this temperature for 8-14 hours.

[0014] The present invention also seeks to protect a 6061 aluminum alloy bar for an automobile probe housing, which is prepared by using the 6061 aluminum alloy bar for an automobile probe housing extrusion process.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] By optimizing the alloy composition, low manganese, low chromium, combined with the online solid solution extrusion process, the appropriate extrusion rod temperature, extrusion ratio and extrusion speed are reasonably set and matched, the recrystallization temperature is reduced by low manganese, low chromium and large extrusion ratio, and a large number of dislocations and sub-grained structures are formed during the extrusion process, which are rapidly recrystallized at the appropriate extrusion rod temperature to form fine recrystallized structures, while preventing the occurrence of secondary recrystallization. Due to the fine recrystallized structure with many interfaces, large deformation resistance, fine grain strengthening effect, and excellent mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The accompanying drawings are used to provide a further understanding of the present invention and are used together with the embodiments of the present invention to explain the present invention, but do not constitute a limitation of the present invention. In the accompanying drawings:

[0018] Figure 1 It is a flow chart of the 6061 aluminum alloy bar extrusion process. DETAILED DESCRIPTION

[0019] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0020] like Figure 1 FIG. 1 is a flow chart of a 6061 aluminum alloy bar extrusion process for an automobile probe housing according to the present invention, comprising the following steps:

[0021] (1) The alloy composition range of the cast rod is optimized as follows: Si: 0.5-0.7%, Cu: 0.2-0.3%, Mg: 0.9-1.0%, Mn<0.05%, Cr: 0.04-0.07%; other additions are made according to national standards, and the rod is cast;

[0022] (2) Take 6061 aluminum alloy bar and heat it;

[0023] (3) Extrusion on the machine, extrusion ratio ≥ 45, extrusion casting temperature 490-515℃, extrusion speed ≥ 5mm / s;

[0024] (4) Online water cooling and solid solution.

[0025] A comparison group of 6061 aluminum alloy bars made by conventional methods and an implementation group of 6061 aluminum alloy bars made by the method of this application are used for comparison. The preparation parameters and performance tests of the two are shown in the following table:

[0026]

[0027]

[0028] The 6061 aluminum alloy rod is prepared by heating and melting the raw materials, alloying, refining, slagging, standing, degassing and filtering, semi-continuous water-cooling casting, homogenizing and water-cooling.

[0029] Extrusion speed refers to the forward speed of the main cylinder of the extruder.

[0030] After online water cooling and solution treatment, the aging temperature is 160-175°C and the temperature is kept for 8-14 hours. In this embodiment, the preferred aging temperature is 165°C and the temperature is kept for 12 hours.

[0031] The present invention also seeks to protect a 6061 aluminum alloy bar for an automobile probe housing, which is prepared by using the 6061 aluminum alloy bar for an automobile probe housing extrusion process.

[0032] From the comparison of the above tables, it is found that by optimizing the alloy composition, low manganese, low chromium, and combining the online solid solution extrusion process, the appropriate extrusion rod temperature, extrusion ratio and extrusion speed are reasonably set and matched, and the recrystallization temperature is reduced by low manganese, low chromium and large extrusion ratio. At the same time, a large number of dislocations and subgrain structures are formed during the extrusion process, and they are rapidly recrystallized at the appropriate extrusion rod temperature to form fine recrystallized structures, while preventing the occurrence of secondary recrystallization. Due to the fine recrystallization structure with many interfaces, large deformation resistance, fine grain strengthening effect, and excellent mechanical properties.

[0033] Finally, it should be noted that the above are only preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or make equivalent substitutions for some of the technical features therein. However, any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A 6061 aluminum alloy bar extrusion process for automobile probe housing, characterized in that: The following steps are involved: (1) The cast rod includes the following alloy components: Si: 0.5-0.7%, Cu: 0.2-0.3%, Mg: 0.9-1.0%, Mn<0.05%, Cr: 0.04-0.07%; other additions are in accordance with national standards; (2) Take 6061 aluminum alloy bar and heat it; (3) Extrusion on the machine, extrusion ratio ≥ 45, extrusion casting temperature 490-515℃, extrusion speed ≥ 5mm / s; (4) Online water cooling and solid solution, The 6061 aluminum alloy rod is prepared by heating and melting the raw materials, alloying, refining, slagging, standing, degassing and filtering, semi-continuous water-cooling casting, homogenizing and water-cooling.

2. The extrusion process of 6061 aluminum alloy bar for automobile probe housing according to claim 1 is characterized in that: Extrusion speed refers to the forward speed of the main cylinder of the extruder.

3. The extrusion process of 6061 aluminum alloy bar for automobile probe housing according to claim 2 is characterized in that: After online water cooling and solution treatment, the aging temperature is 160-175℃ and the temperature is kept at 8-14 hours.

4. A 6061 aluminum alloy bar for automobile probe housing, characterized in that: The automobile probe housing is prepared by the 6061 aluminum alloy bar extrusion process as claimed in any one of claims 1 to 3.

Citation Information

Patent Citations

  • Thermal treatment process of 6061 aluminum alloy

    CN104561859A

  • Process for avoiding coarse-grain rings of 6061 aluminum alloy bars and rods

    CN105256193A

  • Method for preparing 6061 aluminum alloy fine crystalline material

    CN108220842A

  • Extrusion die for aircraft empennage aluminum alloy seamless profile

    CN211613856U

Cited By

  • High-performance modified aluminum alloy material and processing method thereof

    CN121592915A

  • A high-performance modified aluminum alloy material and its processing method

    CN121592915B