Anti-deformation polymer heart valve and preparation method thereof

By surface modification of artificial heart valve fabric substrate, covalent bond fixation sites are formed, the problem of deformation of valves during long-term stress is solved, and the stability and fatigue resistance are significantly improved. It is suitable for artificial heart valves. Application.

CN118987348APending Publication Date: 2024-11-22SHANGHAI HEARTEPOCH MEDICAL TECH CO LTD

Patent Information

Application Number
CN202411118998.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The braided structure of existing artificial heart valves is prone to deformation, contraction, elongation and dispersion when under long-term stress, and lacks stability.

Method used

By surface modification of the fabric substrate, a covalent bond fixing site between the warp yarn and the weft yarn is formed, which enhances the stability of the fabric structure, and uses ultraviolet cross-linking, chemical cross-linking, thermal cross-linking and high-energy ray cross-linking to adopt ultraviolet cross-linking, chemical cross-linking, thermal cross-linking and high-energy ray cross-linking The method is to form stable bond connections.

Benefits of technology

It significantly improves the stability of the leaflets during opening and closing movement, avoids deformation and detachment, enhances fatigue resistance and biocompatibility, and is suitable for use in artificial heart valves.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118987348A_ABST
    Figure CN118987348A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of artificial heart valves, and particularly relates to an anti-deformation high-molecular heart valve and a preparation method thereof.The preparation method comprises the steps that surface modification treatment is conducted on a fabric base material for constructing the high-molecular heart valve, so that covalent bond fixing sites are formed at interweaving points of warp yarn and weft yarn of the fabric base material; the surface modification treatment process of the fabric base material is an ultraviolet light crosslinking process, a chemical crosslinking process, a thermal crosslinking process and / or a high-energy ray crosslinking process. The fabric base material is subjected to surface modification treatment, fixing sites between the warp yarns and the weft yarns are increased, so that the fabric structure is more stable, and the valve leaflets are not prone to shrinkage, extension, disengagement and the like in the opening and closing movement process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of artificial heart valves, and in particular to an anti-deformation polymer heart valve and a preparation method thereof. Background Art

[0002] In recent years, researchers have begun to study the application of biocompatible synthetic polymer materials such as polypropylene, polyurethane, and polyester in artificial heart valves. However, the woven structure of artificial valve fabrics is mostly made of alternating warp and weft yarns. As the base material of the valve leaflet, the fabric is prone to deformation such as shrinkage, elongation, and disintegration when subjected to long-term stress.

[0003] For example, CN108904877A discloses a textile-based polymer valve leaflet in an interventional artificial heart valve based on polymer fiber composite materials and a preparation method thereof. The polymer fiber bundle in its woven structure is composed of M-direction and N-direction fibers, which are arranged in a 1×1 structure, and the acute angle between the M-direction and N-direction fibers is 15 to 30°. The warp and weft yarns are woven alternately, and due to the lack of anchor points, the warp and weft yarns are easily displaced (slipped) and separated during movement, thereby causing fabric deformation and debonding. Summary of the invention

[0004] In view of the defect that woven-based polymer leaflet materials are easily deformed under the action of constant force, the present invention provides a deformation-resistant polymer heart valve and a preparation method thereof. By performing surface modification on the fabric substrate and increasing the fixed points between the warp yarns and the weft yarns, the fabric structure is made more stable, and the leaflets are not easily subject to contraction, elongation, or disintegration during opening and closing movements.

[0005] According to one aspect of the present invention, a method for preparing a deformation-resistant polymer heart valve is provided, the method comprising performing surface modification treatment on a fabric substrate for constructing the polymer heart valve to form covalent bond fixing sites at the interweaving points of the warp yarns and weft yarns of the fabric substrate.

[0006] Preferably, the process of surface modification of the fabric substrate for constructing the polymer heart valve is an ultraviolet light cross-linking process, a chemical cross-linking process, a thermal cross-linking process and / or a high-energy ray cross-linking process.

[0007] Preferably, the UV cross-linking process is to immerse the fabric substrate in an initiator, then irradiate it with UV light, and remove excess initiator after the UV irradiation is completed;

[0008] The chemical cross-linking process is to immerse the fabric substrate in a mixed solution of a silane coupling agent and an initiator, then subject it to a heat treatment to cause a cross-linking reaction, and finally remove the excess initiator;

[0009] The thermal crosslinking process is to expose the amino, hydroxyl and / or carboxyl groups on the surface of the fabric substrate by chemical treatment, and then heat treat the fabric substrate while applying pressure to perform a thermal crosslinking reaction;

[0010] The high-energy ray cross-linking process is to use high-energy rays to treat the interlacing points of the warp yarns and weft yarns of the fabric substrate, so that the polymer surface undergoes radiation cross-linking and forms covalent bond fixing sites between the warp yarns and the weft yarns.

[0011] Preferably, the UV crosslinking process specifically includes: preparing an initiator solution, placing the cleaned fabric substrate into the solution and soaking it for 1 to 2 hours, then taking it out for post-finishing treatment; then irradiating the fabric substrate after post-finishing treatment with UV light having a wavelength of 200 to 400 nm for 1 to 120 minutes; after the irradiation is completed, washing and removing the excess initiator;

[0012] The chemical cross-linking process specifically includes: preparing an initiator solution, adding a silane coupling agent, adding the cleaned fabric substrate and soaking for 1 to 2 hours, and then taking it out for post-finishing treatment; then placing the fabric substrate in an oven at 80 to 100° C. for a cross-linking reaction, and the reaction time is 60 to 120 minutes; after the cross-linking is completed, washing and removing the excess initiator and silane coupling agent;

[0013] The thermal cross-linking process specifically includes: exposing the amino and carboxyl groups on the surface of the fabric substrate by surface carboxylation treatment, then washing and drying, during the drying process, controlling the weight reduction of the fabric to be between 10 and 15%; then subjecting the carboxylation treated fabric to a heat treatment at 150° C. and applying pressure at the same time, so that the carboxyl groups and amino groups at the interlacing points of the warp and weft yarns are cross-linked, and the whole process lasts for 5 to 10 minutes;

[0014] The high-energy ray cross-linking process specifically includes: using electron beams with energy between 3 and 10 kGy to irradiate the interlaced points of the warp and weft yarns of the cleaned fabric substrate, and irradiating each point for 1 to 30 minutes.

[0015] Preferably, in the UV crosslinking process and the chemical crosslinking process,

[0016] The post-finishing treatment is a roller pressing treatment with a pressure of 0.2-2 MPa, or a flat vulcanizing machine is used for treatment, with a controlled temperature of 100-120°C, a pressure of 2-5 MPa and a treatment time of 1-10 min;

[0017] The initiator solution is prepared by dissolving 0.2% to 0.8% of diisopropylbenzene oxide in an organic solvent;

[0018] The mass concentration of the silane coupling agent is 0.2% to 0.6%.

[0019] Preferably, the preparation method further comprises performing a surface coating treatment on the fabric substrate after the surface modification treatment, and the coating material used is an elastic material.

[0020] Preferably, the elastic material is selected from one or a combination of latex, porcine collagen, bovine collagen, elastin, polyether polyurethane, polyester polyurethane, polyurethane urea, styrene rubber, butadiene rubber, isoprene rubber, ethylene propylene rubber, butyl rubber, chloroprene rubber, nitrile rubber, SBS, hydrogenated SBS, SIS, hydrogenated SIS, ethylene-octene copolymer, thermoplastic vulcanized rubber and polyamide thermoplastic elastomer;

[0021] And / or, the elastic modulus of the elastic material is 2-40 MPa, and the elongation at break is between 100% and 700%.

[0022] Preferably, the fabric substrate is made by weaving or knitting, wherein the weaving structure is any one of a warp flat structure, a warp flat velvet structure and a warp satin structure, and the warp density is 100 to 400 strands / inch, and the weft density is 100 to 400 strands / inch; and / or,

[0023] The fabric substrate is made of at least one of polypropylene, polyethylene terephthalate, polyamide, high molecular weight polyethylene, ultra-high molecular weight polyethylene, aramid, polyester polyurethane and polyether polyurethane; and / or,

[0024] The fabric base material is made of multifilament fiber, the denier is 10D-40D, and the number of multifilaments is between 6f and 72f.

[0025] Preferably, the preparation method further comprises a final molding process, that is, cutting and molding the surface-modified fabric substrate using a laser according to a leaflet drawing or using a specific knife die.

[0026] According to another aspect of the present invention, there is further provided a deformation-resistant polymer heart valve, which is manufactured using the above-mentioned preparation method.

[0027] The present invention adopts the above technical solution to have at least the following beneficial effects:

[0028] 1. The anti-deformation polymer heart valve and preparation method thereof provided by the present invention, by surface modification treatment of the fabric substrate, a number of fixed sites are formed at the interlacing points of the warp yarn and the weft yarn in the form of covalent bonds, so that the fabric structure is more stable, and the valve leaflets are not easy to shrink, stretch, or fall apart during the opening and closing movement;

[0029] 2. The deformation-resistant polymer heart valve and preparation method thereof provided by the present invention can form covalent bond fixing sites on the surface of the fabric substrate by ultraviolet irradiation, thereby enhancing the stability and fatigue resistance of the fabric, and ultraviolet crosslinking is a clean and fast surface treatment method without the need to use a large amount of chemical reagents; a silane coupling agent and an initiator can be used to cause a crosslinking reaction under heat treatment to enhance the bonding force between the warp and weft yarns of the fabric. This method can achieve high-strength crosslinking in a relatively short period of time and is suitable for large-scale production; amino, hydroxyl, carboxyl and other groups on the surface of the fabric substrate can be exposed and crosslinked by heat treatment to form stable chemical bonds. This method can achieve high-efficiency crosslinking at a relatively low cost and is suitable for various types of polymer materials; high-energy rays can also be used to treat the warp and weft interlacing points of the fabric substrate to achieve radiation crosslinking. This method can achieve crosslinking without contacting the fabric, avoiding the use of chemicals, and is an environmentally friendly treatment method;

[0030] 3. The deformation-resistant polymer heart valve and its preparation method provided by the present invention can provide additional biocompatibility and mechanical strength through the coating process. The coating can further enhance the fatigue resistance and deformation resistance of the fabric and improve its performance in biomedical applications;

[0031] 4. The deformation-resistant polymer heart valve and its preparation method provided by the present invention use fiber materials such as polypropylene, polyester, etc. that have good biocompatibility and biodegradability, as well as high strength and fatigue resistance; they are suitable for making fabric substrates for artificial heart valves. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of a weaving pattern of a fabric substrate according to an embodiment of the present invention. DETAILED DESCRIPTION

[0033] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the present application. The various commonly used reagents used in the examples are all commercially available products.

[0034] Example 1

[0035] Weaving: The polyester woven fabric layer is prepared with polyethylene terephthalate fiber. The yarn used is 40D / 72f multifilament yarn. The structure is warp-plain structure. The warp density is 120 strands / inch and the weft density is 110 strands / inch. The weaving pattern of the obtained fabric base material is referenced Figure 1 As shown;

[0036] Cleaning and drying: 40g / L sodium carbonate, 10g / L sodium hydroxide, clean at 80℃ for 20min, then wash and dry;

[0037] Padding: prepare an initiator, diisopropylbenzene oxide, 0.2% to 0.8%, and dissolve it in a xylene solution; then put the cleaned polyester fabric in and soak it for 1 to 2 hours, then take it out and treat it with a pressure roller (pressure 0.2 to 2 MPa);

[0038] Ultraviolet irradiation: irradiate the taken-out fabric with ultraviolet light of wavelength between 200 and 400 nm for 1 to 120 minutes;

[0039] Cleaning: After irradiation, use xylene to clean out excess initiator, and then use ethanol and purified water to clean in sequence;

[0040] Coating: dip-coating the fabric after irradiation cleaning with 1% porcine collagen / acetic acid solution for 2 to 5 times, then taking it out and drying it, so as to obtain a non-deformable polymer leaflet material;

[0041] Forming: Cut the fabric into the shape of petals using a specific die.

[0042] Example 2

[0043] Weaving: The woven fabric is made of ultra-high molecular weight polyethylene fiber, the yarn used is 10D / 12f multifilament yarn, the structure is warp flat velvet structure, the warp density is 180 strands / inch, and the weft density is 180 strands / inch;

[0044] Cleaning and drying: 40g / L sodium carbonate, 10g / L sodium hydroxide, clean at 80℃ for 20min, then wash and dry;

[0045] Soaking: prepare 0.2% to 0.8% of the initiator diisopropylbenzene oxide and dissolve it in a xylene solution, then add 0.2% to 0.6% of a silane coupling agent; then put the cleaned ultra-high molecular weight polyethylene fabric in and soak it for 1 to 2 hours and then take it out;

[0046] Leveling: Treat the soaked ultra-high molecular weight polyethylene fabric with a flat vulcanizer at 100-120 degrees Celsius, 2-5 MPa, and time of 1-10 minutes;

[0047] Cross-linking reaction: the above fabric is placed in an oven at 80-100°C for reaction for 60-120 minutes;

[0048] Cleaning: After cross-linking is completed, use xylene to clean out excess initiator and silane coupling agent, and then use ethanol and purified water to clean in turn;

[0049] Coating: dip-coating the fabric after irradiation cleaning with a 10% polyurethane solution for 1 to 5 times, then taking it out and drying it, thereby obtaining a deformation-resistant ultra-high molecular weight polyethylene leaflet material;

[0050] Forming: Cut the fabric into the shape of petals using a specific die.

[0051] Example 3

[0052] Weaving: The woven fabric is made of polypropylene fiber, the yarn used is 20D / 24f multifilament yarn, the structure is warp satin structure, the warp density is 160 strands / inch, and the weft density is 160 strands / inch;

[0053] Cleaning and drying: 40g / L sodium carbonate, 10g / L sodium hydroxide, clean at 80℃ for 20min, then wash and dry;

[0054] Electron beam irradiation: Use electron beams with energy between 3 and 10 kGy to irradiate the warp and weft interlacing points of the polypropylene fabric. Each point is irradiated for 1 to 30 minutes. After the time is up, the polypropylene leaflets that resist deformation can be obtained by taking them out.

[0055] Forming: Cut the fabric into the shape of petals using a specific die.

[0056] Example 4

[0057] Weaving: The woven fabric is made of polyamide fiber, the yarn used is 30D / 36f multifilament yarn, the structure is warp flat structure, the warp density is 100 strands / inch, and the weft density is 100 strands / inch;

[0058] Surface carboxylation treatment: 40g / L sodium hydroxide, washing at 100℃ for 60min, the purpose is to hydrolyze the polymer, expose the surface amino and carboxyl groups, and then wash and dry. The weight of the fabric will decrease after washing, and the reduction is controlled between 10 and 15%;

[0059] Thermal crosslinking: The carboxylated fabric is heat treated at 150 degrees Celsius and pressurized at the same time to allow the carboxyl and amino groups at the interlacing points of the warp and weft yarns to form crosslinks. The whole process lasts for 5 to 10 minutes.

[0060] Molding: It is preferred to use laser cutting to cut and shape according to the leaflet drawing, because the heat generated by laser cutting will promote the thermal cross-linking of the carboxyl and amino groups on the surface of the nearby yarns, or use a specific knife die to cut the fabric into the shape of the leaflet.

[0061] Comparative Example 1: The same as Example 1, except that the padding, ultraviolet irradiation and cleaning steps are missing.

[0062] Comparative Example 2: The same as Example 2, except that the soaking, leveling, cross-linking and cleaning steps are missing.

[0063] Table 1 Leaflet fatigue test results of different schemes

[0064] name Fatigue times Fatigue results Example 1 50 million times The leaflets are not deformed and the edges are not loose Example 2 200 million times The leaflets are not deformed and the edges are not loose Example 3 200 million times The leaflets are not deformed and the edges are not loose Example 4 200 million times The leaflets are not deformed and the edges are not loose Comparative Example 1 50 million times The leaflets are deformed and the edges are partially dislocated Comparative Example 2 200 million times The leaflets are deformed and the edges are loose

[0065] The test method for leaflet fatigue performance is carried out in accordance with the valve fatigue test method in ISO 5840-1 (GB 12279-2008). The samples prepared in the examples / comparative examples are sewn to the corresponding nickel-titanium valve frame of 23mm specification, and then placed on the valve fatigue equipment for testing. Parameters: frequency 15Hz, transvalvular pressure difference 90-120mmHg, liquid temperature 37℃±1℃. Every 5 million times, the edge dislocation or deformation of the leaflet is observed and recorded by a high-speed camera. After the fatigue test, the valve is taken out and the morphology of the valve leaflet is observed under an optical microscope to see if deformation, shrinkage, dislocation, etc. occur.

[0066] From the above results, it can be seen that after the surface modification treatment of the fabric substrate in Examples 1-4 of the present invention, the covalent bond fixing sites formed at the interweaving points of the warp yarn and the weft yarn enhance the fatigue resistance of the fabric, allowing the leaflets to remain stable under cyclic stretching, significantly extending the fatigue life.

[0067] It should be noted that the above description is only a detailed description of the preferred embodiments and principles of the present invention. For ordinary technicians in this field, there will be changes in the specific implementation methods based on the ideas provided by the present invention, and these changes should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a deformation-resistant polymer heart valve, characterized in that: The preparation method comprises performing surface modification treatment on a fabric substrate for constructing a polymer heart valve, so as to form a covalent bond fixing site at the interweaving point of the warp yarn and the weft yarn of the fabric substrate.

2. The preparation method according to claim 1, characterized in that: The process of surface modification of the fabric substrate for constructing the polymer heart valve is an ultraviolet light cross-linking process, a chemical cross-linking process, a thermal cross-linking process and / or a high-energy ray cross-linking process.

3. The preparation method according to claim 2, characterized in that: The UV cross-linking process is to immerse the fabric substrate in an initiator, then irradiate it with UV light, and remove the excess initiator after the UV irradiation is completed. The chemical cross-linking process is to immerse the fabric substrate in a mixed solution of a silane coupling agent and an initiator, then subject it to a heat treatment to cause a cross-linking reaction, and finally remove the excess initiator; The thermal crosslinking process is to expose the amino, hydroxyl and / or carboxyl groups on the surface of the fabric substrate by chemical treatment, and then heat treat the fabric substrate while applying pressure to perform a thermal crosslinking reaction; The high-energy ray cross-linking process is to use high-energy rays to treat the interlacing points of the warp yarns and weft yarns of the fabric substrate, so that the polymer surface undergoes radiation cross-linking and forms covalent bond fixing sites between the warp yarns and the weft yarns.

4. The preparation method according to claim 3, characterized in that: The ultraviolet crosslinking process specifically includes: preparing an initiator solution, placing the cleaned fabric substrate into the solution and soaking it for 1 to 2 hours, then taking it out for post-finishing treatment; then irradiating the fabric substrate after post-finishing treatment with ultraviolet light having a wavelength of 200 to 400 nm for 1 to 120 minutes; after the irradiation is completed, washing and removing the excess initiator; The chemical cross-linking process specifically includes: preparing an initiator solution, adding a silane coupling agent, adding the cleaned fabric substrate and soaking for 1 to 2 hours, and then taking it out for post-finishing treatment; then placing the fabric substrate in an oven at 80 to 100° C. for a cross-linking reaction, and the reaction time is 60 to 120 minutes; after the cross-linking is completed, washing and removing the excess initiator and silane coupling agent; The thermal cross-linking process specifically includes: exposing the amino and carboxyl groups on the surface of the fabric substrate by surface carboxylation treatment, then washing and drying, during the drying process, controlling the weight reduction of the fabric to be between 10 and 15%; then subjecting the carboxylation treated fabric to a heat treatment at 150° C. and applying pressure at the same time, so that the carboxyl groups and amino groups at the interlacing points of the warp and weft yarns are cross-linked, and the whole process lasts for 5 to 10 minutes; The high-energy ray cross-linking process specifically includes: using electron beams with energy between 3 and 10 kGy to irradiate the interlaced points of the warp and weft yarns of the cleaned fabric substrate, and irradiating each point for 1 to 30 minutes.

5. The preparation method according to claim 4, characterized in that: In the UV crosslinking process and the chemical crosslinking process, The post-finishing treatment is a roller pressing treatment with a pressure of 0.2-2 MPa, or a flat vulcanizing machine is used for treatment, with a controlled temperature of 100-120°C, a pressure of 2-5 MPa and a treatment time of 1-10 min; The initiator solution is prepared by dissolving 0.2% to 0.8% of diisopropylbenzene oxide in an organic solvent; The mass concentration of the silane coupling agent is 0.2% to 0.6%.

6. The preparation method according to claim 1, characterized in that: The preparation method further comprises performing surface coating treatment on the fabric substrate after the surface modification treatment, and the coating material used is an elastic material.

7. The preparation method according to claim 6, characterized in that: The elastic material is selected from one or a combination of latex, porcine collagen, bovine collagen, elastin, polyether polyurethane, polyester polyurethane, polyurethane urea, styrene rubber, butadiene rubber, isoprene rubber, ethylene propylene rubber, butyl rubber, chloroprene rubber, nitrile rubber, SBS, hydrogenated SBS, SIS, hydrogenated SIS, ethylene-octene copolymer, thermoplastic vulcanized rubber and polyamide thermoplastic elastomer; And / or, the elastic modulus of the elastic material is 2-40 MPa, and the elongation at break is between 100% and 700%.

8. The preparation method according to claim 1, characterized in that: The fabric substrate is made by weaving or knitting, wherein the weaving structure is any one of a warp plain structure, a warp flat velvet structure and a warp satin structure, and the warp density is 100 to 400 strands / inch, and the weft density is 100 to 400 strands / inch; and / or, The fabric substrate is made of at least one of polypropylene, polyethylene terephthalate, polyamide, high molecular weight polyethylene, ultra-high molecular weight polyethylene, aramid, polyester polyurethane and polyether polyurethane; and / or, The fabric base material is made of multifilament fiber, the denier is 10D-40D, and the number of multifilaments is between 6f and 72f.

9. The preparation method according to claim 1, characterized in that: The preparation method also includes a final molding process, that is, cutting and molding the surface-modified fabric substrate using a laser according to a leaflet drawing or using a specific knife die.

10. A deformation-resistant polymer heart valve, characterized in that: The preparation method is adopted according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of pure-wool fabric

    CN110725045A

  • Anti-wrinkle real silk fabric and preparation method thereof

    CN113338033A

  • N,N-bis(2-acrylamidoethyl)acrylamide as well as preparation method and application thereof

    CN113861059A

  • Low-leakage textile-based composite valve leaflet and processing method thereof

    CN116159180A

  • Stabilized fabric material for medical devices

    US20210045868A1

Cited By

  • Preparation system of high-elasticity and high-strength artificial heart valve leaflet

    CN120753832A

  • System for preparing high-elastic high-strength artificial heart valve leaflets

    CN120753832B