Electrolytic aluminum cathode assembly structure, casting assembly platform and casting assembly method
By using a combination method of argon buffer chamber and heating device in electrolytic aluminum cathode assembly, the high energy consumption and oxidation problems of the electrolytic aluminum cathode assembly method of phosphorus pig iron cast electrolytic aluminum cathode assembly method are solved, the conductivity and bond reliability of the cathode are improved, and the More efficient production process.
Patent Information
- Application Number
- CN202411134738.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing phosphorus pig iron cast electrolytic aluminum cathode assembly method has problems such as high energy consumption, easy oxidation of cathode carbon blocks and cathode steel rods, and easy falling off during handling and use, which affects the cathode conductivity and production efficiency.
Using an electrolytic aluminum cathode casting assembly platform and method, the high temperature oxidation is avoided through the argon buffer chamber and heating device, and the non-uniform expansion deformation is used to improve the bonding reliability of the cathode carbon block, the cathode steel rod and the phosphorus pig iron layer, including the hollow rectangular type The box, pallet, side support device and heating device control the temperature through argon blowing and heating device, form a local low oxygen environment and undergo non-uniform expansion and deformation to enhance the connection.
It reduces energy consumption, avoids high-temperature oxidation, improves the conductivity of the cathode, and enhances the bonding reliability between the cathode carbon block, cathode steel rod and phosphorus pig iron layer, and improves the production efficiency and service life of the cathode.
Smart Images

Figure CN118905207A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrolytic aluminum, and in particular to an electrolytic aluminum cathode assembly structure, a casting assembly platform and a casting assembly method. Background Art
[0002] Modern electrolytic aluminum production mainly adopts cryolite-alumina molten salt electrolysis, which uses molten cryolite as solvent, alumina as solute, carbonite as anode, and aluminum liquid as cathode. After a strong direct current is passed, an electrochemical reaction is carried out at the two electrodes in the electrolytic cell at 950℃-970℃. The phosphorus pig iron cast electrolytic aluminum cathode composed of cathode carbon block, cathode steel rod and phosphorus pig iron connecting cathode carbon block and cathode steel rod is one of the important parts of electrolytic aluminum equipment.
[0003] At present, the phosphorus pig iron casting electrolytic aluminum cathode assembly method requires that the cathode carbon block and the cathode steel rod be assembled in position to form a cathode group, and the assembled cathode group is then preheated as a whole by natural gas or electricity, and phosphorus pig iron molten iron is cast at a certain temperature to achieve the assembly purpose. However, this assembly method also has the following defects:
[0004] (1) A large amount of energy is consumed in the process of assembling the cathode carbon block and the cathode steel rod and then preheating them as a whole.
[0005] (2) During the overall preheating process of the cathode carbon block and cathode steel rod process group, the temperature is high, and it is difficult to completely isolate the air. It is inevitable that the cathode carbon block and cathode steel rod will be oxidized before casting, and the oxide layer will directly affect the conductivity of the cathode in the later electrolytic aluminum production.
[0006] (3) After the cast phosphorus pig iron is cast, the cathode steel rod is very likely to fall off from the cathode carbon block during transportation and use due to its large mass, which reduces the cathode manufacturing efficiency of the aluminum electrolytic cell and increases costs. Summary of the invention
[0007] In order to solve the problems of high energy consumption and easy oxidation of cathode carbon blocks and cathode steel bars in the existing phosphorus pig iron casting electrolytic aluminum cathode assembly method, the present invention provides an electrolytic aluminum cathode assembly structure, a casting assembly platform and a casting assembly method, which avoid high-temperature oxidation to ensure the conductivity of the later electrolytic aluminum cathode, and at the same time improve the reliability of the combination between the cathode carbon block, the cathode steel bar and the phosphorus pig iron layer by utilizing the non-uniform expansion deformation of the cathode carbon block.
[0008] The technical solution adopted by the present invention is:
[0009] An electrolytic aluminum cathode casting assembly platform, comprising:
[0010] A box body, wherein the box body is in the shape of a hollow rectangular parallelepiped with an open top; along the height direction of the box body, the projection of the box body completely includes the projection of the electrolytic aluminum cathode;
[0011] A support plate, the support plate is located above the bottom of the box body, and its length and width are smaller than the corresponding length and width of the inner side of the box body; an argon buffer chamber is formed between the support plate and the inner bottom of the box body; and a gap between the support plate and the inner side wall of the box body forms an annular argon blowing port;
[0012] Side support devices, the side support devices have four units, two of each unit forms a group; two side support devices in the same group are respectively arranged on the side walls of the box body on the opposite length side, and are used to support the side wall of the cathode carbon block of the electrolytic aluminum cathode by surface contact;
[0013] A heating device, which has four units and is used to heat cathode steel rods of electrolytic aluminum cathodes;
[0014] The thin sheet has a thickness of 0.05-0.1 mm and is randomly laid on the contact surface between the side support device and the electrolytic aluminum cathode.
[0015] Furthermore, the width of the annular argon blowing port is 0.5-2 mm.
[0016] Furthermore, a side wall of the box body is provided as an openable door; and a pulley is provided on the lower surface of the support plate.
[0017] Furthermore, the inner bottom surface of the box body and the lower surface of the support plate are provided with matching slide grooves and slide plates, and a part of the slide plate is located in the slide groove and can slide back and forth along the length direction of the slide groove.
[0018] Furthermore, baffles are respectively arranged on both sides of the length direction of the upper surface of the support plate; the two baffles are arranged along the width direction of the support plate, and the distance between them is the length of the cathode carbon block of the electrolytic aluminum cathode.
[0019] Furthermore, the side support device includes a side pressure plate and a hydraulic cylinder, the side pressure plate is located in the box body and is parallel to the side wall on the length side of the box body; the hydraulic cylinder is located on the outside of the box body, and its working end passes through the corresponding side wall of the box body and is connected to the side pressure plate.
[0020] Furthermore, the heating device comprises a ceramic shell and an electric heating rod, one side of the ceramic shell is open; and the electric heating rod is arranged inside the ceramic shell along the length direction of the ceramic shell.
[0021] A method for casting and assembling an electrolytic aluminum cathode is implemented based on the aforementioned electrolytic aluminum cathode casting and assembly platform, and comprises the following steps:
[0022] Step S1, placing the cathode carbon block and cathode steel rod assembly on a support plate in the box;
[0023] Step S2, introducing argon into the argon buffer chamber and releasing it from the annular argon blowing port;
[0024] Step S3, after passing argon gas for 10 to 20 minutes, start the heating device to heat the cathode steel rod, and monitor the temperature of the lower part of the cathode steel rod in the U-shaped through groove; when the temperature of the lower part of the cathode steel rod in the U-shaped through groove reaches 200 to 250° C., continue heating for 10 to 20 minutes, and stop heating;
[0025] Step S4, casting the molten phosphorus pig iron into the gap between the cathode steel rod and the slot wall of the U-shaped through slot, forming a phosphorus pig iron layer after cooling, stopping the introduction of argon gas, and obtaining the electrolytic aluminum cathode assembly structure.
[0026] An electrolytic aluminum cathode assembly structure is manufactured by the electrolytic aluminum cathode casting assembly method as described above, comprising:
[0027] A cathode carbon block, wherein the cathode carbon block is in a rectangular shape, and two U-shaped through grooves are opened on the top surface thereof in parallel along the length direction of the cathode carbon block; and the groove wall of the U-shaped through groove is a non-smooth and flat surface;
[0028] A U-shaped plug, the U-shaped plug is arranged in the U-shaped through groove;
[0029] A cathode steel rod, wherein the cathode steel rod is arranged in the U-shaped through groove, one end of the cathode steel rod abuts against the U-shaped plug; the other end of the cathode steel rod is located outside the U-shaped through groove; there is a gap between the surface of the cathode steel rod and the adjacent wall of the U-shaped through groove;
[0030] A phosphorus pig iron layer is located in the gap between the surface of the cathode steel rod and the adjacent wall of the U-shaped through groove.
[0031] Furthermore, a groove is provided on the surface of the corresponding portion of the cathode steel rod located in the U-shaped through groove.
[0032] The beneficial effects of the present invention are:
[0033] The present invention discloses an electrolytic aluminum cathode assembly structure, a casting assembly platform and a casting assembly method, which avoid high-temperature oxidation to ensure the conductivity of the later electrolytic aluminum cathode, and improve the reliability of the combination between the cathode carbon block, the cathode steel rod and the phosphorus pig iron layer by utilizing the non-uniform expansion deformation of the cathode carbon block. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 This is a front view of the electrolytic aluminum cathode in Example 1.
[0036] Figure 2 for Figure 1 AA section view.
[0037] Figure 3 Schematic diagram of the three-dimensional structure of the electrolytic aluminum cathode in Example 1.
[0038] Figure 4 Schematic diagram of the structure of the electrolytic aluminum cathode casting assembly platform in Example 2 Figure 1 .
[0039] Figure 5 Schematic diagram of the structure of the electrolytic aluminum cathode casting assembly platform in Example 2 Figure 2 .
[0040] Figure 6 Schematic diagram of the exploded structure of the electrolytic aluminum cathode casting assembly platform in Example 2.
[0041] Figure 7 Schematic diagram of the process of casting and assembling the electrolytic aluminum cathode in Example 3.
[0042] The accompanying drawings are marked as follows:
[0043] 100-cathode carbon block, 110-U-shaped through slot;
[0044] 200-U-type plug;
[0045] 300- cathode steel rod;
[0046] 400-phosphorus pig iron layer;
[0047] 500-box body, 510-box door, 520-support plate, 521-argon gas buffer chamber, 522-annular argon gas blowing port, 523-pulley, 524-blocking bar, 530-slideway, 540-slide plate;
[0048] 600-side support device, 610-side pressure plate, 620-hydraulic cylinder;
[0049] 700-thin slices;
[0050] 800-heating device, 810-ceramic housing. DETAILED DESCRIPTION
[0051] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0052] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention.
[0053] The embodiments of the invention are described in detail below with reference to the accompanying drawings.
[0054] Example 1
[0055] Figure 1 This is a front view of the electrolytic aluminum cathode in Example 1. Figure 2 for Figure 1 AA section view. Figure 3 Schematic diagram of the three-dimensional structure of the cathode of aluminum electrolysis in Example 1. Figures 1 to 3 As shown in , the electrolytic aluminum cathode assembly structure includes a rectangular cathode carbon block 100. Two U-shaped through grooves 110 are opened in parallel on the top surface of the cathode carbon block 100 along the length direction of the cathode carbon block 100. A U-shaped plug 200 adapted to the U-shaped through groove 110 is arranged in the middle of the inner length direction of each U-shaped through groove 110, and the U-shaped plug 200 is made of fireproof cotton or the like. The U-shaped plug 200 cuts the U-shaped through groove 110 into two parts with approximately equal groove lengths. A cathode steel rod 300 is also respectively arranged in the two parts of the U-shaped through groove 110 cut off by the U-shaped plug 200. One end of the cathode steel rod 300 abuts against the U-shaped plug 200, and the other end of the cathode steel rod 300 is located outside the U-shaped through groove 110. Meanwhile, between the surface of the cathode steel rod 300 and the groove wall of the adjacent U-shaped through groove 110 is a phosphorus pig iron layer 400 formed after the phosphorus pig iron molten iron is cast and cooled.
[0056] In this embodiment, the groove wall of the U-shaped groove 110 has randomly distributed micro-protrusions and micro-depressions, that is, the groove wall of the U-shaped groove 110 is a non-smooth and flat surface. During the cooling process of the phosphorus pig iron molten iron casting, the phosphorus pig iron layer 400 forms micro-depressions and micro-protrusions that match the randomly distributed micro-protrusions and micro-depressions on the groove wall of the U-shaped groove 110, thereby increasing the reliability of the connection between the phosphorus pig iron layer 400 and the cathode carbon block 100 and reducing the risk of separation of the cathode carbon block 100 and the cathode steel rod 300.
[0057] In this embodiment, a groove (not shown) is provided on the surface of the corresponding portion of the cathode steel rod 300 located in the U-shaped through groove 110, and the phosphorus pig iron layer 400 can penetrate into the groove, thereby increasing the tightness of the connection between the two.
[0058] Example 2
[0059] Figure 4 Schematic diagram of the structure of the electrolytic aluminum cathode casting and assembly platform used for casting and assembling the electrolytic aluminum cathode in Example 1 in Example 2 Figure 1 . Figure 5 Schematic diagram of the structure of the electrolytic aluminum cathode casting and assembly platform used for casting and assembling the electrolytic aluminum cathode in Example 1 in Example 2 Figure 2 . Figure 6 Schematic diagram of the exploded structure of the electrolytic aluminum cathode casting and assembly platform used for casting and assembling the electrolytic aluminum cathode in Example 1 in Example 2. Figure 4 ~Attached Figure 6As shown in , the cathode casting and assembly platform of the electrolytic furnace includes a box 500 with a hollow rectangular structure. The top of the box 500 is open; at the same time, the length and width of the inner side of the box 500 meet the requirements of accommodating the cathode of electrolytic aluminum, that is, along the height direction of the box 500, the projection of the cathode of electrolytic aluminum is completely located within the projection of the box 500. The internal space of the box 500 is the main space for casting and assembling the cathode of electrolytic aluminum. An argon gas interface is provided at the bottom of the box 500, and a rectangular support plate 520 is provided in parallel near the bottom of the inner side of the box 500. The support plate 520 is mainly used to support the cathode of electrolytic aluminum. The length and width of the support plate 520 are smaller than the inner length and width of the corresponding box 500. For example, there is a gap of 0.5~2mm between the edges of the support plate 520 and the inner side walls of the adjacent box 500. The distance between the upper surface of the support plate 520 and the open top surface of the box 500 is roughly equal to the height of the cathode carbon block. In this embodiment, an argon buffer chamber 521 is formed between the support plate 520 and the inner bottom of the box body 500, and a gap between the support plate 520 and the inner side wall of the box body 500 forms an annular argon blowing port 522. In this embodiment, by controlling the amount of argon entering the argon buffer chamber 521, the amount of argon released from the annular argon blowing port 522 can be regulated to form a local low oxygen area (the volume concentration of oxygen in the local low oxygen area is less than 20%) at the inner edge of the box body 500 and the surrounding internal space, and the high temperature oxidation effect can be reduced when the electrolytic aluminum cathode is cast and assembled in the local low oxygen area.
[0060] In this embodiment, the electrolytic aluminum cathode casting assembly platform also includes four side support devices 600. The four side support devices 600 are grouped in pairs and are respectively arranged on the side walls of the opposite length of the box body 500. Each side support device 600 is against the side wall of the length of the cathode carbon block 100 corresponding to the cathode steel rod 300 from the top to the area below the bottom of the U-shaped through groove 110 through surface contact. The two side support devices 600 in the same group provide certain lateral support to the cathode carbon block 100 in the width direction to prevent the cathode carbon block 100 from being damaged by heat expansion. At the same time, the contact surface between the side support device 600 and the cathode carbon block 100 is also randomly laid with a number of thin sheets 700 with a thickness of 0.05~0.1mm. The shape of the thin sheet 700 can be regular shapes such as regular circles and squares, or irregular shapes such as C-shaped and S-shaped. During the thermal expansion of the cathode carbon block 100, the side support device 600 provides a certain lateral pressure in the reverse direction. At the same time, due to the randomly laid thin sheets 700, the reverse pressure on the cathode carbon block 100 is non-uniform, which accelerates the non-uniform expansion and deformation of the groove wall area of the U-shaped groove 110, forming randomly distributed micro-protrusions and micro-depressions, that is, the groove wall of the U-shaped groove 110 forms a non-smooth and flat surface.
[0061] In this embodiment, the electrolytic aluminum cathode casting assembly platform also includes four heating devices 800. The four heating devices are respectively placed on the top of the four cathode steel rods 300 to heat the cathode steel rods 300 and preheat them to a set temperature. At the same time, the heated cathode steel rods 300 increase the temperature of the groove wall of the U-shaped groove 110 through heat radiation, change the local temperature of the cathode carbon block 100, and are beneficial to the casting process of phosphorus pig iron. At the same time, during the heating process of the groove wall area of the U-shaped groove 110, it expands and deforms non-uniformly under the action of uneven reverse pressure, forming randomly distributed micro-protrusions and micro-depressions, that is, the groove wall of the U-shaped groove 110 forms a non-smooth and flat surface. During the cooling process of casting molten phosphorus pig iron, the phosphorus pig iron layer 400 forms micro-depressed portions and micro-protrusions that cooperate with the micro-protrusions and micro-depressed portions randomly distributed on the groove wall of the U-shaped through groove 110, thereby increasing the reliability of the connection between the phosphorus pig iron layer 400 and the cathode carbon block 100 and reducing the risk of separation of the cathode carbon block 100 and the cathode steel rod 300.
[0062] In this embodiment, the side wall on one side of the width of the box body 500 is set as an openable box door 510. At the same time, a number of pulleys 523 are evenly arranged on the lower surface of the support plate 520. As a result, the support plate 520 and the electrolytic aluminum cathode carried thereon can easily enter and exit the box body 500. Further, in this embodiment, a matching chute 530 and a slide plate 540 are arranged on the inner bottom surface of the box body 500 and the lower surface of the support plate 520. A part of the slide plate 540 is located in the chute 530 and can slide back and forth along the length direction of the chute 540, so that the support plate 520 can quickly slide into the box body 500 along the set direction to avoid the influence of left and right shaking on the electrolytic aluminum cathode. In this embodiment, in order to avoid the chute 530 and the slide plate 540 blocking the argon gas, a plurality of argon gas interfaces can be provided, and the plurality of argon gas interfaces are respectively located on both sides of the chute 530.
[0063] In this embodiment, the baffles 524 are respectively arranged on both sides of the upper surface of the support plate 520 in the length direction, and the baffles 524 are arranged along the width direction of the support plate 520, and the cathode carbon block 100 is clamped between the two baffles 524, that is, the length direction of the cathode carbon block 100 is consistent with the length direction of the support plate 520, and the length of the cathode carbon block 100 is equal to the distance between the two baffles 524. In this embodiment, the baffles 524 can limit the sliding of the cathode carbon block 100 in the length direction, and can also play a role in installation and positioning.
[0064] In this embodiment, the side support device 600 includes a side pressure plate 610 and a plurality of hydraulic cylinders 620 working synchronously. The side pressure plate 610 is located in the box body 500, and is roughly parallel to the side wall of the box body 500 on one side of the length. The hydraulic cylinder 620 is located outside the box body 500, and its working end passes through the corresponding side wall of the box body 500 and is connected to the side pressure plate 610. In this embodiment, the position of the side pressure plate 610 and the force applied by the side pressure plate 610 to the cathode carbon block 100 can be adjusted by the hydraulic cylinder 620.
[0065] In this embodiment, the heating device 800 includes a ceramic shell 810 and an electric heating rod. One side of the ceramic shell 810 is open, and the length of the ceramic shell 810 is about 4 / 5 of the length of the cathode steel rod 300. The electric heating rod is arranged inside the ceramic shell 810 along the length direction of the ceramic shell 810. When in use, the heating device 800 is placed on the top of the cathode steel rod 300 along the length direction of the cathode steel rod 300, and the open edge of the ceramic shell 810 contacts the top surface of the cathode steel rod 300, and then the electric heating rod can be energized to heat the cathode steel rod 300. The heated cathode steel rod 300 can heat up the groove wall area of the U-shaped groove 110 of the cathode carbon block 100 through heat radiation, and expand and deform in an uneven manner under the uneven reverse pressure provided by the lateral support device 600, forming randomly distributed micro-protrusions and micro-depressions, that is, the groove wall of the U-shaped groove 110 forms a non-smooth and flat surface. In this embodiment, the cathode carbon block 100 and the cathode steel rod 300 are not preheated as a whole. Instead, the heating device 800 is used to directly heat the cathode steel rod 300 and indirectly heat the cathode carbon block 100, thereby reducing power consumption.
[0066] Example 3
[0067] Figure 7 Schematic diagram of the process of the electrolytic aluminum cathode casting and assembly method in Example 3 based on the electrolytic aluminum cathode casting and assembly platform in Example 2. Figure 7 As shown, the electrolytic aluminum cathode casting and assembly method comprises the following steps:
[0068] Step S1, placing the cathode carbon block 100 on the support plate 520, installing the U-shaped plug 200, and then placing the cathode steel rods 300 one by one into the U-shaped groove 110 of the cathode carbon block 100, and then moving the combined structure of the cathode steel rod 300 and the cathode carbon block 100 into the box body 500, and then closing the box door 510, adjusting the side support device 600 to press against the side wall of the cathode carbon block 100 and randomly inserting a thin sheet 700 with a thickness of 0.08 mm in the process of the side support device 600 gradually pressing against the cathode carbon block 100; wherein, the gap between the cathode steel rod 300 and the groove wall of the U-shaped groove 110 is formed by placing a number of supporting steel blocks in the U-shaped groove 110 in advance, and then placing them into the U-shaped groove 110; the thin sheet 700 can also be first connected to the side support device 600 by pasting;
[0069] Step S2, continuously introducing argon into the argon buffer chamber 521 formed by the box body 500 and the support plate 520, so that the argon is released from the annular argon blowing port 522 with a gap of 1 mm until the casting and assembly of the electrolytic aluminum cathode is completed;
[0070] Step S3, after passing argon gas for 10 to 20 minutes, start the heating device 800 to heat the cathode steel rod 300, and monitor the temperature of the lower part of the cathode steel rod 300 in the U-shaped through groove 110; when the temperature of the lower part of the cathode steel rod 300 in the U-shaped through groove 110 reaches 200 to 250° C. (for example, 200° C.), continue heating for 10 to 20 minutes (for example, 15 minutes), and then stop heating;
[0071] Step S4, casting the molten phosphorus pig iron (temperature of 1350-1450°C) into the gap between the cathode steel rod 300 and the slot wall of the U-shaped through slot 110 one by one, gradually cooling to form a phosphorus pig iron layer 400, stopping the introduction of argon gas, and obtaining the electrolytic aluminum cathode assembly structure.
[0072] The electrolytic aluminum cathode casting and assembly method in this embodiment can reduce energy consumption, avoid high-temperature oxidation and ensure the conductivity of the electrolytic aluminum cathode in the later stage. At the same time, the non-uniform expansion and deformation of the cathode carbon block is utilized to improve the reliability of the bonding between the cathode carbon block, the cathode steel rod and the phosphorus pig iron layer.
Claims
1. An electrolytic aluminum cathode casting assembly platform, It is characterized in that include: A box body, wherein the box body is in the shape of a hollow rectangular parallelepiped with an open top; along the height direction of the box body, the projection of the box body completely includes the projection of the electrolytic aluminum cathode; A support plate, the support plate is located above the bottom of the box body, and its length and width are smaller than the corresponding length and width of the inner side of the box body; an argon buffer chamber is formed between the support plate and the inner bottom of the box body; and a gap between the support plate and the inner side wall of the box body forms an annular argon blowing port; Side support devices, the side support devices have four units, two of each unit forms a group; two side support devices in the same group are respectively arranged on the side walls of the box body on the opposite length side, and are used to support the side wall of the cathode carbon block of the electrolytic aluminum cathode by surface contact; A heating device, which has four units and is used to heat cathode steel rods of electrolytic aluminum cathodes; The thin sheet has a thickness of 0.05-0.1 mm and is randomly laid on the contact surface between the side support device and the electrolytic aluminum cathode.
2. The electrolytic aluminum cathode casting assembly platform according to claim 1, It is characterized in that The width of the annular argon blowing port is 0.5-2 mm.
3. The electrolytic aluminum cathode casting assembly platform according to claim 1, It is characterized in that A side wall of one side of the box body is arranged as an openable box door; and a pulley is arranged on the lower surface of the support plate.
4. The electrolytic aluminum cathode casting assembly platform according to claim 3, It is characterized in that The inner bottom surface of the box body and the lower surface of the support plate are provided with matching slide grooves and slide plates, and a part of the slide plate is located in the slide groove and can slide back and forth along the length direction of the slide groove.
5. The electrolytic aluminum cathode casting assembly platform according to claim 1, It is characterized in that Baffles are respectively arranged on both sides of the upper surface of the support plate in the length direction; the two baffles are arranged along the width direction of the support plate, and the distance between them is the length of the cathode carbon block of the electrolytic aluminum cathode.
6. The electrolytic aluminum cathode casting assembly platform according to any one of claims 1 to 5, It is characterized in that The side support device includes a side pressure plate and a hydraulic cylinder. The side pressure plate is located in the box body and is parallel to the side wall on the length side of the box body. The hydraulic cylinder is located on the outside of the box body, and its working end passes through the corresponding side wall of the box body and is connected to the side pressure plate.
7. The electrolytic aluminum cathode casting assembly platform according to any one of claims 1 to 5, It is characterized in that The heating device comprises a ceramic shell and an electric heating rod. One side of the ceramic shell is open; the electric heating rod is arranged inside the ceramic shell along the length direction of the ceramic shell.
8. A method for casting and assembling an electrolytic aluminum cathode, which is implemented based on the electrolytic aluminum cathode casting and assembly platform as described in any one of claims 1 to 7. It is characterized in that The following steps are involved: Step S1, placing the cathode carbon block and cathode steel rod assembly on a support plate in the box; Step S2, introducing argon into the argon buffer chamber and releasing it from the annular argon blowing port; Step S3, after passing argon gas for 10 to 20 minutes, start the heating device to heat the cathode steel rod, and monitor the temperature of the lower part of the cathode steel rod in the U-shaped through groove; when the temperature of the lower part of the cathode steel rod in the U-shaped through groove reaches 200 to 250° C., continue heating for 10 to 20 minutes, and stop heating; Step S4, casting the molten phosphorus pig iron into the gap between the cathode steel rod and the slot wall of the U-shaped through slot, forming a phosphorus pig iron layer after cooling, stopping the introduction of argon gas, and obtaining the electrolytic aluminum cathode assembly structure.
9. An electrolytic aluminum cathode assembly structure, made by the electrolytic aluminum cathode casting assembly method according to claim 8, It is characterized in that include: A cathode carbon block, wherein the cathode carbon block is in a rectangular shape, and two U-shaped through grooves are opened on the top surface thereof in parallel along the length direction of the cathode carbon block; and the groove wall of the U-shaped through groove is a non-smooth and flat surface; A U-shaped plug, the U-shaped plug is arranged in the U-shaped through groove; A cathode steel rod, wherein the cathode steel rod is arranged in the U-shaped through groove, one end of the cathode steel rod abuts against the U-shaped plug; the other end of the cathode steel rod is located outside the U-shaped through groove; there is a gap between the surface of the cathode steel rod and the adjacent wall of the U-shaped through groove; A phosphorus pig iron layer is located in the gap between the surface of the cathode steel rod and the adjacent wall of the U-shaped through groove.
10. The electrolytic aluminum cathode assembly structure according to claim 9, It is characterized in that A groove is formed on the surface of the corresponding portion of the cathode steel rod located in the U-shaped through groove.