Metal powder hot isostatic pressing forming process based on graphite sheath and application of metal powder hot isostatic pressing forming process
By using a hot isostatic pressing process that combines graphite sheathing with ceramic particles, the issues of precision and cost in manufacturing complex-shaped parts have been resolved. This process achieves high-precision, low-cost near-net-shape forming, simplifies the sheathing removal process, and improves the forming effect of the parts.
Patent Information
- Application Number
- CN202411164631.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-08
AI Technical Summary
Existing hot isostatic pressing (HIP) processes have problems in manufacturing complex-shaped parts, such as low part accuracy, high cost, difficulty in making and removing the sheath, and the inability to apply excessively high HIP temperatures. In particular, there are shortcomings in conformal outer steel sheath, inner steel core shape control, inner graphite core shape control, and ceramic mold sheath processes.
A graphite cladding with a porosity of 30-35% is combined with metal powder. By filling the graphite cladding with ceramic particles and performing hot isostatic pressing, the uniform shrinkage of the graphite cladding and the pressure transmission properties of the ceramic particles are utilized to achieve dense forming of the metal powder, simplifying the cladding removal process and reducing ceramic inclusions.
It improves the precision and purity of the parts, reduces production costs, simplifies the casing removal process, enhances the forming effect and yield of complex-shaped parts, and meets high-performance requirements.
Smart Images

Figure CN118905222A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder metallurgy, and in particular relates to a metal powder hot isostatic pressing process based on graphite sheathing and an application thereof. Background Art
[0002] The hot isostatic pressing near-net forming process is widely used in the manufacture of complex-shaped parts. The existing main forming processes include conformal outer steel sleeve forming, inner steel core controlled forming, inner graphite core controlled forming, and ceramic mold sleeve forming. Among them, the conformal outer steel sleeve forming process is widely used because of its simple manufacturing and low cost, but it is only suitable for the near-net forming of relatively simple blanks. It is difficult to achieve precise control of the shape for parts with complex shapes, and irregular shrinkage may occur after forming. It is necessary to reserve a certain amount of processing allowance to ensure the accuracy of the final shape. The inner steel core controlled forming process is mainly used to accurately control the shape of the internal cavity of the part. For parts with complex inner cavity shapes, chemical corrosion is usually required to remove the steel core, which is costly and inefficient. In addition, the corrosive liquid may have a harmful effect on the part, and due to the high-temperature strength of the steel core, it is impossible to achieve too fine control of the shape. Although the inner graphite core controlled forming process is easy to process and remove, it is impossible to accurately control the shape of the inner cavity due to the certain porosity of graphite. After the graphite is densified by pretreatment, a forming core can be made for shape control, but the external shape of the part still needs to be machined.
[0003] The hot isostatic pressing formed by combining the processes of conformal outer steel sleeve forming, inner steel core controlled forming, inner graphite core controlled forming, etc. can improve the forming accuracy of the parts to a certain extent, but it still cannot avoid the disadvantages of each forming, resulting in high production costs, difficulty in sleeve production, difficulty in sleeve removal, large processing allowance of parts, and the hot isostatic pressing temperature should not be too high.
[0004] Ceramic mold sleeve forming process is an advanced hot isostatic pressing near-net forming technology. Although domestic research institutions such as Central South University and Beijing Institute of Aeronautical Materials have conducted relevant research, the preparation technology of ceramic mold sleeves is very complicated, and there has been no successful case of near-net forming using this process. In addition, ceramic inclusions are easily introduced during the production process of ceramic mold sleeves, affecting product quality. Therefore, it is urgent to provide a metal powder hot isostatic pressing forming process to solve the problems of part forming after the combination of processes such as conformal outer steel sleeves, inner steel core shape control, and inner graphite core shape control, as well as the problems existing in the ceramic mold sleeve forming process.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a metal powder hot isostatic pressing process based on graphite sheathing and its application, aiming to overcome the above-mentioned technical problems and provide a process with lower cost, higher part precision and easy to achieve near-net forming.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] On the one hand, the present invention provides a metal powder hot isostatic pressing process based on graphite sheathing, and the specific steps are as follows:
[0009] S1. Design and manufacture a graphite sheath that matches the enlarged size of the workpiece shape. The graphite sheath is made of a graphite block with a porosity of 30 to 35% and a wall thickness of 5 to 8 mm.
[0010] S2. Put metal powder for forming parts into graphite sheath and seal it by shaking. The particle size of the metal powder is 15-250μm. The metal powder includes but is not limited to one of titanium alloy powder, nickel-based powder and iron-based powder. Among them, titanium alloy powder is metal powder with nickel-iron content less than 1.5%, and the grades are TC4, TC11, TA15, TC21, TC18, TA2, etc.; nickel-based powder is metal powder with nickel content higher than 50%, and the grades are GH4169, GH4099, FGH4097, GH3536, GH3625, GH3230, etc.; iron-based powder is metal powder with iron content higher than 70%, and the grades are 304, 316L, 18Ni300, 17-4PH, etc.; when the metal powder is nickel-based or iron-based powder, a layer of pure nickel needs to be electroplated on the inner surface of the graphite sheath, and the thickness of the electroplated pure nickel layer is 0.5-1mm;
[0011] S3, placing the sealed graphite sheath in the center of the metal sheath, and filling the gap between the graphite sheath and the metal sheath with ceramic particles, wherein the particle size of the ceramic particles is 0.1 to 0.8 mm;
[0012] S4, vacuuming, heating, degassing and sealing the filled metal sheath;
[0013] S5, subjecting the sealed metal sheath to hot isostatic pressing, wherein the hot isostatic pressing temperature is 850-1200° C., the pressure is 100-150 MPa, and the holding time is 2-5 h;
[0014] S6, removing the metal sheath and breaking the ceramic particles;
[0015] S7. By machining or crushing away the graphite sheath, a near-net-shape part can be obtained.
[0016] Furthermore, during the hot isostatic pressing process, the graphite sheath is used to provide a space for uniform shrinkage, ensuring the shape of the final product after shrinkage. The ceramic particles, based on their fluidity and high temperature resistance, are used to uniformly transfer the pressure of the steel sheath to the graphite sheath during the forming process. The final effect is that the outer steel sheath shrinks under pressure, and the pressure transmitted by the ceramic particles causes the graphite sheath to shrink, thereby making the metal powder densely formed.
[0017] On the other hand, the present invention provides an application of the metal powder hot isostatic pressing process based on graphite sheathing as described above, wherein the metal powder hot isostatic pressing process based on graphite sheathing is applied to the near-net forming of complex-shaped parts or parts with high performance requirements.
[0018] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0019] The metal powder hot isostatic pressing process of the present invention effectively solves the problem of accurate forming of complex-shaped parts by designing the combined use of graphite sheaths and metal sheaths, reduces the problem of irregular shrinkage caused by the complex shape of parts in traditional methods, and improves the adaptability of the dimensional accuracy and shape complexity of parts; by adopting the easy-to-remove characteristics of ceramic particle filling and graphite sheaths, it not only simplifies the removal process of the sheath, but also effectively reduces the ceramic inclusions that may be introduced during the hot isostatic pressing process, and improves the purity and yield rate of the parts; the surface of the parts formed by this process has high dimensional accuracy and good surface roughness, which meets the use requirements of most parts. The present invention significantly enhances the application effect of hot isostatic pressing technology in the manufacture of complex-shaped parts, improves the cost-effectiveness ratio and the quality of parts, and provides an effective solution to solve the pain points of the industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0022] Figure 1 It is a schematic diagram of the process flow of the present invention.
[0023] Among them: 1 is a graphite sheath; 2 is metal powder; 3 is a graphite sheath cover; 4 is a metal sheath; 5 is ceramic particles; 6 is a metal sheath upper plate; 7 is a degassing port; and 8 is a formed part. DETAILED DESCRIPTION
[0024] Here, exemplary embodiments will be described in detail, and examples thereof are shown in the accompanying drawings. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples consistent with some aspects of the present invention as detailed in the appended claims.
[0025] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0026] Example 1
[0027] See also Figure 1 As shown, this embodiment provides a metal powder hot isostatic pressing process based on graphite sheathing, and the specific steps are as follows:
[0028] Step 1: According to the shape of the disc-shaped workpiece, the tap density of the TC4 powder, and the hot isostatic pressing dimensional shrinkage coefficient, the inner size shape of the graphite sheath 1 before shrinkage is designed, and the graphite sheath 1 is made of a graphite block with a porosity of 30%. The wall thickness of the graphite sheath 1 is 5 mm.
[0029] Step 2: Load TC4 metal powder 2 into the graphite sheath 1 and compact it using a vibration table. The powder weight is calculated to be 30 kg based on the volume and the powder compaction density. The actual powder weight is 30.1 kg. Cover it with a graphite sheath cover 3 to seal it. The particle size range of the titanium alloy metal powder used is 50 to 150 μm.
[0030] Step 3: Use low-carbon steel material to weld and make the metal sheath 4, first fill a certain thickness of ceramic particles 5 at the bottom of the metal sheath 4, then place the sealed graphite sheath 1 above the ceramic particles 5, ensure that the graphite sheath 1 is basically located at the center of the metal sheath 4, and continue to fill the ceramic particles 5 into the metal sheath 4 until the metal sheath 4 is filled. The material of the ceramic particles 5 is Al2O3, and the particle size of the ceramic particles 5 is 0.5mm. The metal sheath upper plate 6 is welded to the upper part of the filled metal sheath 4.
[0031] Step 4: Place the welded metal sheath 4 in a vacuum electron beam heating degassing device for vacuum degassing. When the vacuum degree inside the metal sheath 4 is 5*10 -4 After Pa, the degassing port 7 is sealed by electron beam welding.
[0032] Step 5: The sealed metal sheath 4 is subjected to hot isostatic pressing treatment, the hot isostatic pressing temperature is 920° C., the pressure is 120 MPa, and the insulation time is 2.5 h.
[0033] Step 6: Use mechanical processing to remove the outer metal sheath 4 and the metal sheath upper plate 6, and break the coating layer of the ceramic particles 5 to obtain the shrunk graphite sheath 1.
[0034] Step 7: Use mechanical processing to remove the graphite sheath 1 to obtain the final formed part 8. The dimensional control accuracy of the formed part 8 is ±0.1. The formed part 8 does not need secondary processing to meet the dimensional requirements, and the part can be formed in one step near net shape.
[0035] The prepared TC4 product has a tensile strength of 945 MPa, a yield strength of 885 MPa, an elongation of 18%, a dimensional deviation of ±0.1 mm, and a surface roughness better than Ra2.4, all of which meet the use requirements of the product.
[0036] Example 2
[0037] See also Figure 1 As shown, this embodiment provides a metal powder hot isostatic pressing process based on graphite sheathing, which is specifically carried out according to the following steps:
[0038] Step 1: According to the shape of the disc-shaped workpiece, the tap density of the GH4169 powder, and the hot isostatic pressing dimensional shrinkage coefficient, the inner size shape of the graphite sheath 1 before shrinkage is designed, and the graphite sheath 1 is made of a graphite block with a porosity of 35%. The wall thickness of the graphite sheath 1 is 8 mm.
[0039] Step 2: Load GH4169 metal powder 2 into graphite sheath 1 and vibrate it using a vibration table. The powder weight is calculated to be 40 kg by volume and powder tap density, and the actual powder weight is 40.5 kg. Cover the sheath with a graphite sheath cover 3 to seal it. The particle size range of the GH4169 metal powder used is 15 to 113 μm. In order to prevent the diffusion of carbon atoms into the GH4169 matrix at high temperature of graphite, a pure nickel coating with a thickness of 0.8 mm is electroplated on the inner surface of the graphite sheath 1.
[0040] Step 3: Use low-carbon steel material to weld and make the metal sheath 4, first fill a certain thickness of ceramic particles 5 at the bottom of the metal sheath 4, then place the sealed graphite sheath 1 above the ceramic particles 5, ensure that the graphite sheath 1 is basically located at the center of the metal sheath 4, and continue to fill the ceramic particles 5 into the metal sheath 4 until the metal sheath 4 is filled. The material of the ceramic particles 5 is Al2O3, and the particle size of the ceramic particles 5 is 0.8mm. The metal sheath upper plate 6 is welded to the upper part of the filled metal sheath 4.
[0041] Step 4: Place the welded metal sheath 4 in a vacuum electron beam heating degassing device for vacuum degassing. When the vacuum degree inside the metal sheath 4 is 5*10 -4 After Pa, the degassing port 7 is sealed by electron beam welding.
[0042] Step 5: The sealed metal sheath 4 is subjected to hot isostatic pressing treatment, the hot isostatic pressing temperature is 1150° C., the pressure is 130 MPa, and the insulation time is 3.5 h.
[0043] Step 6: Use mechanical processing to remove the outer metal sheath 4 and the metal sheath upper plate 6, and break the coating layer of the ceramic particles 5 to obtain the shrunk graphite sheath 1.
[0044] Step 7: Remove the graphite sheath 1 by knocking to obtain the final formed part 8. The dimensional control accuracy of the formed part 8 is ±0.2. The formed part 8 does not need to be processed again to meet the dimensional requirements, and the part can be formed in one step near net shape.
[0045] The prepared GH4169 product has a tensile strength of 1419 MPa, a yield strength of 1185 MPa, an elongation of 19%, a dimensional deviation of ±0.2 mm, and a surface roughness better than Ra2.4, all of which meet the use requirements of the product.
[0046] Example 3
[0047] See also Figure 1 As shown, this embodiment provides a metal powder hot isostatic pressing process based on graphite sheathing, which is specifically carried out according to the following steps:
[0048] Step 1: According to the shape of the disc-shaped workpiece, the tap density of the 18Ni300 powder, and the hot isostatic pressing dimensional shrinkage coefficient, the inner size shape of the graphite sheath 1 before shrinkage is designed, and the graphite sheath 1 is made of a graphite block with a porosity of 33%. The wall thickness of the graphite sheath 1 is 7 mm.
[0049] Step 2: Load 18Ni300 metal powder 2 into graphite sheath 1 and vibrate it using a vibration table. The powder weight is calculated to be 40 kg by volume and powder compaction density, and the actual powder weight is 40.1 kg. Cover the sheath with a graphite sheath cover 3 to seal it. The particle size range of the 18Ni300 metal powder used is 15 to 113 μm. In order to prevent the diffusion of carbon atoms into the 18Ni300 matrix at high temperatures of graphite, a pure nickel coating with a thickness of 1 mm is electroplated on the inner surface of the graphite sheath 1.
[0050] Step 3: Use low-carbon steel material to weld and make the metal sheath 4, first fill a certain thickness of ceramic particles 5 at the bottom of the metal sheath 4, then place the sealed graphite sheath 1 above the ceramic particles 5, ensure that the graphite sheath 1 is basically located at the center of the metal sheath 4, and continue to fill the ceramic particles 5 into the metal sheath 4 until the metal sheath 4 is filled. The material of the ceramic particles 5 is Al2O3, and the particle size of the ceramic particles 5 is 0.2mm. The metal sheath upper plate 6 is welded to the upper part of the filled metal sheath 4.
[0051] Step 4: Place the welded metal sheath 4 in a vacuum electron beam heating degassing device for vacuum degassing. When the vacuum degree inside the metal sheath 4 is 4.3*10 -4 After Pa, the degassing port 7 is sealed by electron beam welding.
[0052] Step 5: The sealed metal sheath 4 is subjected to hot isostatic pressing treatment, the hot isostatic pressing temperature is 1180° C., the pressure is 130 MPa, and the insulation time is 3.5 h.
[0053] Step 6: Use mechanical processing to remove the outer metal sheath 4 and the metal sheath upper plate 6, and break the coating layer of the ceramic particles 5 to obtain the shrunk graphite sheath 1.
[0054] Step 7: Remove the graphite sheath 1 by knocking to obtain the final formed part 8. The dimensional control accuracy of the formed part 8 is ±0.2. The formed part 8 does not need to be processed again to meet the dimensional requirements, and the part can be formed in one step near net shape.
[0055] The prepared 18Ni300 parts have a tensile strength of 1730 MPa, a yield strength of 1650 MPa, an elongation of 10.5%, a dimensional deviation of ±0.2 mm, and a surface roughness better than Ra2.4, all of which meet the use requirements of the parts.
[0056] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0057] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A metal powder hot isostatic pressing process based on graphite sheathing, characterized in that: The specific steps are as follows: S1. Design and manufacture graphite sheaths that match the enlarged size of the workpiece; S2, putting metal powder for forming parts into the graphite sleeve and sealing it by shaking; S3, placing the sealed graphite sheath at the center of the metal sheath, and filling the gap between the graphite sheath and the metal sheath with ceramic particles; S4, vacuuming, heating, degassing and sealing the filled metal sheath; S5, subjecting the sealed metal sheath to hot isostatic pressing; S6, remove the metal sheath and break the ceramic particles; S7. By machining or crushing away the graphite sheath, a near-net-shape part can be obtained.
2. The metal powder hot isostatic pressing process according to claim 1, characterized in that: The particle size of the metal powder is 15 to 250 μm.
3. The metal powder hot isostatic pressing process according to claim 1, characterized in that: The metal powder includes but is not limited to one of titanium alloy powder, nickel-based powder and iron-based powder.
4. The metal powder hot isostatic pressing process according to claim 3, characterized in that: In step 2, when the metal powder is nickel-based or iron-based powder, a layer of pure nickel needs to be electroplated on the inner surface of the graphite sheath.
5. The metal powder hot isostatic pressing process according to claim 4, characterized in that: The thickness of the electroplated pure nickel layer is 0.5 to 1 mm.
6. The metal powder hot isostatic pressing process according to claim 1, characterized in that: In step 1, the graphite sheath is made of a graphite block with a porosity of 30-35%.
7. The metal powder hot isostatic pressing process according to claim 1, characterized in that: In step 1, the wall thickness of the graphite sheath is 5 to 8 mm.
8. The metal powder hot isostatic pressing process according to claim 1, characterized in that: In step 3, the particle size of the ceramic particles is 0.1 to 0.8 mm.
9. The metal powder hot isostatic pressing process according to claim 1, characterized in that: In step 5, the hot isostatic pressing temperature is 850-1200° C., the pressure is 100-150 MPa, and the holding time is 2-5 hours.
10. Application of the metal powder hot isostatic pressing process according to any one of claims 1 to 9, characterized in that: The metal powder hot isostatic pressing process is applied to the near-net-shape forming of parts with complex shapes or parts requiring high performance.
Citation Information
Patent Citations
Hot isostatic pressing integrated forming method of complex part with special functional layer
CN104972114A
Hot isostatic pressing forming method used for improving part surface quality
CN105436505A
Method for controlling size of powder high-temperature high-entropy alloy blade
CN118417566A
Automobile bearing manufacturing installation
CN207359294U
Method and arrangement for manufacturing a component with hot isostatic pressing, a core, a preform for a cladding, and use of the core
US20130202476A1
Cited By
Preparation process of composite gradient material based on additive manufacturing-hot isostatic pressing
CN121928050A