Copper-steel bimetallic antifriction plate and preparation method thereof

By filling the copper alloy layer of copper steel bimetallic sheet with carbonized substances and using the high-temperature decomposition reaction of polymer compounds, the safety hazards of lead and graphite and poor interfacial bonding quality in copper steel bimetallic sheet are solved, and the materials are improved The friction-reducing properties and mechanical properties reduce the lead content and enhance the hardness.

CN118905226APending Publication Date: 2024-11-08合肥波林新材料股份有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410952556.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The use of lead and graphite as friction reducing components in existing copper and steel bimetallic materials has safety hazards and poor interface bonding quality, which affects the mechanical and tribological properties of the material.

Method used

The microstructure of the copper alloy layer has pores and is filled with polymer compounds or mixtures as impregnation agents. The friction reduction performance is improved through the carbonized substances decomposed after high temperature, and the surface density and hardness are increased through two sintering and two rolling processes. Impregnation and carbonization are performed in the pores of the copper alloy layer.

Benefits of technology

The friction reduction and mechanical properties of copper-steel bimetallic sheets are improved, the lead content is reduced, the deformation influence of graphite during the rolling process is avoided, and the hardness and interface quality of the sheets are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905226A_ABST
    Figure CN118905226A_ABST
Patent Text Reader

Abstract

The invention provides a copper-steel bimetallic antifriction plate and a preparation method thereof.The copper-steel bimetallic antifriction plate comprises a base body and a copper alloy layer, the base body is made of an iron-based material, and the copper alloy layer is made of a copper alloy sintering material; the microstructure of the copper alloy layer is provided with pores, the pores are filled with carbonization substances, and the carbonization substances are solid products obtained after infiltration of an infiltration agent and high-temperature decomposition. According to the sintered copper-steel bimetal plate, the microstructure of the copper alloy layer is provided with the pores, the impregnant permeates into the pores of the copper alloy layer and is heated and carbonized, the impregnant is heated and decomposed, the pores of the copper alloy layer are filled with the carbonized substances, and therefore the antifriction effect of the plate is improved. In addition, when the copper-steel double-metal plate reaches the same friction coefficient, the lead content in the copper-steel double-metal plate can be reduced, and therefore the influence on the human body is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of sintered metal plates, and in particular relates to a copper-steel bimetallic anti-friction plate and a preparation method thereof. Background Art

[0002] Copper-steel bimetallic materials, generally steel is the base layer, which has the high strength and high hardness of steel, and copper is the working layer, which has the anti-seizure, anti-friction and corrosion resistance of copper. It is widely used in many industries and has formed some specifications and standards. For example, GB13238-1991 "Copper-steel composite steel plate" stipulates that copper-steel composite steel plates with a total thickness of 8 to 30 mm are suitable for the manufacture of corrosion-resistant pressure vessels and vacuum equipment in chemical, petroleum and other industries; JB / T 4115-2022 "Sintered bimetallic plates for side plates of hydraulic pumps and hydraulic motors" stipulates the manufacture of powder metallurgy sintered side plates or oil distribution plate plates suitable for hydraulic pumps and hydraulic motors.

[0003] Sintered metal sheets generally require a working layer (copper surface) with good friction reduction performance, such as the two copper alloy surface materials specified in JB / T 4115-2022 and JB / T 4115-1999, namely 01 / 02, with lead contents of 4%-8% and 7%-10% respectively. Lead is used as a friction reduction component, but lead is a heavy metal and is harmful to the human body, and may harm the human blood circulation system, digestive system and nervous system, etc., so its use should be minimized. In addition, graphite is also a commonly used friction reduction component. If graphite is directly added to the copper alloy layer, common problems such as those pointed out in patent document CN106756214A will occur: graphite has poor wettability with the copper matrix, poor interface bonding quality, pores at the interface bonding, and severe matrix splitting, which will weaken the mechanical properties and tribological properties of the material. CN106756214A prepares graphite into copper-plated graphite and adds it to the copper alloy layer. However, graphite will also affect the rolling process. That is, during rolling, the copper alloy layer will undergo a large plastic deformation, and the graphite in the pores will also deform, splitting the matrix and affecting the interface quality and mechanical properties. Summary of the invention

[0004] The purpose of the present invention is to provide a copper-steel bimetallic anti-friction sintered carbonized plate and a preparation method thereof, so as to improve the anti-friction performance of the copper-steel bimetallic plate.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] The first inventive object of the present invention is to provide a copper-steel bimetallic anti-friction plate, comprising a substrate and a copper alloy layer, wherein the substrate is an iron-based material, and the copper alloy layer is a copper alloy sintered and rolled material; the microstructure of the copper alloy layer has pores, and the pores are filled with carbides, and the carbides are solid products after the infiltration of the infiltrant and high-temperature decomposition.

[0007] In a further embodiment, the impregnating agent is a polymer compound or a mixture, and the carbonized material is filled into the pores to a depth of ≥0.1 mm.

[0008] The second object of the present invention is to provide a method for preparing the above-mentioned copper-steel bimetallic anti-friction sintered carburized plate, comprising the following steps:

[0009] S1. preparing a sintered copper-steel bimetallic sheet;

[0010] In a further embodiment, the preparation steps of the sintered copper-steel bimetallic sheet include:

[0011] S11, spreading the copper alloy powder on the surface of the base steel plate;

[0012] S12, performing the first sintering in a protective atmosphere;

[0013] S13, performing a first rolling on the green body after the first sintering;

[0014] S14, placing the green body after the first rolling in a sintering furnace for a second sintering;

[0015] S15, rolling the blank after the second sintering for the second time to obtain a plate blank; that is, a sintered copper-steel bimetallic plate is obtained.

[0016] In a further embodiment, the base steel plate is a low carbon steel plate, such as 15 steel in GB / T 699-1999 and Q355 steel in GB / T1591-2018; after the second rolling, a leveling machine is used for leveling.

[0017] The sintered copper-steel bimetallic plate of the present invention needs to be sintered twice and rolled twice during the preparation process, wherein the purpose of the first rolling is to increase the density of the surface layer, and the rolling amount is 30-40% of the thickness of the copper alloy layer in the first sintered blank; since the first rolling will cause large deformation between the powders and there will be large deformation stress, the purpose of the second sintering is to remove the stress and further increase the bonding between the powder particles; the purpose of the second rolling is to increase the density of the surface layer and increase the smoothness of the surface layer; the rolling amount is 10-15% of the thickness of the copper alloy layer in the second sintered blank.

[0018] In the present application, the temperature of the first sintering and the second sintering is 800-850° C., and the heat preservation time is 10-40 minutes.

[0019] S2, infiltration treatment: infiltrating an infiltrant into the pores of the copper alloy layer in the sintered copper-steel bimetallic plate, wherein the infiltrant is a polymer compound or a mixture;

[0020] In a further embodiment, the infiltration depth of the infiltration agent into the pores of the copper alloy layer is ≥0.1 mm.

[0021] In a further solution, the impregnant is a liquid impregnant; the sintered copper-steel bimetallic sheet is placed in an impregnation box, vacuumed, and then the liquid impregnant is injected to allow the impregnant to enter the pores of the copper alloy layer; or the sintered copper-steel bimetallic sheet is placed in the liquid impregnant and soaked for 3-60 minutes to allow the impregnant to enter the pores of the copper alloy layer.

[0022] S3. Carbonization: Heating to the carbonization temperature to carbonize the infiltrant in the pores of the copper alloy layer to obtain a sintered copper-steel bimetallic sintered carbide sheet.

[0023] In a further embodiment, the heating to the carbonization temperature means first heating to 70°C-150°C in a water bath, air or protective atmosphere for curing, and then raising the temperature to the carbonization temperature to carbonize the impregnant, wherein the carbonization temperature is 300°C-600°C.

[0024] That is, first heat to the solidification temperature of the liquid infiltrant to solidify the liquid infiltrant in the pores of the sintered copper-steel bimetallic sheet; then continue to heat or keep warm for a period of time or continue to heat after cooling to increase the temperature to the carbonization temperature to carbonize the infiltrant.

[0025] Since the liquid infiltrant has penetrated into the pores of the sintered copper-steel bimetallic sheet, the heating process during the carbonization process is a slow heating process, and the heating rate is ≤12℃ / min. When passing through the curing temperature range, the infiltrant will solidify and there is no need for specific insulation settings or water bath heating.

[0026] The carbonization process of the impregnant is a process in which a polymer compound or a mixture is decomposed by heat, that is, the polymer compound or the mixture is decomposed by heat, losing all or part of substances such as O and H, leaving part of the solid C or a combination of C.

[0027] The liquid infiltrant described in the present application contains a curing agent and is a commercially available infiltrant for powder metallurgy products or castings, such as Permaseal C-2005 infiltrant, GODER-1890 infiltrant, and the like.

[0028] The third invention objective of the present invention is to provide the use of the copper-steel bimetallic anti-friction plate for preparing mechanical parts, including but not limited to rolled sleeves, vane pump or plunger pump oil distribution plates, gear pump side plates. After the carbonization process, the mechanical parts may also include a leveling process, an oil immersion process, a shaping process, and a machining process.

[0029] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0030] 1. The sintered copper-steel bimetallic plate of the present application is composed of a base steel plate and a copper alloy layer, wherein the base steel plate has no pores, while the microstructure of the copper alloy layer has pores. The infiltrant is infiltrated into the pores of the copper alloy layer and heated to carbonize, so that the infiltrant is decomposed by heat, and the pores of the copper alloy layer are filled with carburized substances, thereby improving the friction reduction effect of the plate.

[0031] 2. The present application is to infiltrate the pores of the copper alloy layer of the sintered copper-steel bimetallic plate into the infiltrant and heat it for carbonization. Compared with the prior art of directly adding graphite to the copper alloy powder to achieve friction reduction, the plate has better friction reduction performance and mechanical properties. This is because graphite is added to the copper alloy powder and mixed to form a mixed powder, and then a powder spreading machine is used to spread the copper alloy powder mixed with graphite powder on the surface of the steel plate (such as the powder spreading machine for bimetallic composite materials disclosed in the authorization announcement number CN101327476B). Since the density of graphite is relatively small, it is usually 2.05-2.35g / cm 3 , while the density of copper alloy is relatively large (the density of copper alloy is usually about 8.5-9.0g / cm 3 ), so when spreading the powder, the graphite falls slowly, causing the graphite to float on the surface of the copper alloy, which can easily cause graphite segregation.

[0032] Even if copper-plated graphite powder is used, such as Cu60 copper-plated graphite powder, the copper content is 60wt%, the graphite content is 40wt%, and the graphite density is 2.2g / cm 3 , the density of copper is 8.9g / cm 3 Calculation shows that the density of Cu60 copper-coated graphite is 4.01 g / cm 3 The density of Cu60 copper-plated graphite is significantly lower than that of copper alloy, which will also cause graphite to float on the surface of copper alloy and produce graphite segregation.

[0033] 3. The present application has undergone two sintering and two rolling processes when preparing the sintered copper-steel bimetallic sheet, thereby increasing the density of the copper alloy layer while removing the surface deformation stress. The infiltrant is then infiltrated into the pores of the copper alloy layer of the sintered copper-steel bimetallic sheet and heated to carbonize, thereby increasing the hardness and friction reduction performance of the sheet. In addition, the present application allows the infiltrant to infiltrate the pores of the copper alloy layer after the secondary rolling process and then carbonizes it, so it will not affect the rolling process, and the carbon formed after carbonization remains in the pores to enhance the hardness of the sheet and improve the mechanical properties of the sheet.

[0034] In the prior art, graphite is made into copper-plated graphite and then added to the copper alloy layer (CN106756214A). The graphite will affect the rolling process. That is, during rolling, the copper alloy layer will undergo a large plastic deformation, and the graphite in the pores will also deform, splitting the matrix and affecting the interface quality and mechanical properties.

[0035] 4. The preparation method of the present application can reduce the lead content in the copper-steel bimetallic plate while achieving the same friction coefficient, thereby reducing the impact on the human body.

[0036] 5. The impregnation agent in the present application is a polymer compound or a mixture, which will decompose when heated during the carbonization process. The polymer compound or the mixture will decompose when heated, lose all or part of O and H, and leave a part of solid C or a combination of C.

[0037] In the present application, the carbonization temperature is 300°C-600°C. If the carbonization temperature is too high, more free activated carbon will be formed at high temperature, and the amount of carbon left in the pores will be very small, thus affecting the friction reduction effect; at the same time, if the temperature is too high, the plate may be deformed, and if the temperature is too high, energy consumption will increase, which is not conducive to cost control; if the carbonization temperature is low, the infiltrant in the pores of the sintered matrix is ​​not easy to carbonize. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is the organization diagram of the carbonized material prepared in Example 2;

[0039] Figure 2 The carbon component distribution in the material structure of Example 2;

[0040] Figure 3 This is the distribution of copper components in the material structure of Example 2. DETAILED DESCRIPTION

[0041] The present invention is further described in detail below with reference to the embodiments.

[0042] Embodiment 1:

[0043] The preparation method of the copper-steel bimetallic anti-friction plate comprises the following steps:

[0044] S1. Preparation of sintered copper-steel bimetallic sheet:

[0045] Prepare steel plates and copper alloy powder, wherein the copper alloy powder is CuCn6Zn3Pb6 powder, and the steel plates are low-carbon steel plates No. 15 steel with a thickness of 2.5 mm.

[0046] S11, spreading the copper alloy powder on the surface of the base steel plate;

[0047] S12, placing in a sintering furnace under a protective atmosphere for the first sintering, the sintering temperature is 820°C, and the temperature is kept for 30 minutes; cooling in the furnace to obtain a primary sintered blank;

[0048] S13, rolling the primary sintered billet for the first time to obtain a primary rolled billet; the purpose of the first rolling is to increase the density of the surface layer, and the rolling amount is 30% of the thickness of the copper alloy layer in the primary sintered billet;

[0049] S14, placing the first rolled billet in a sintering furnace for a second sintering, the sintering temperature is controlled at 830° C., the duration is 20 min, and then cooling with the furnace to obtain a second sintered billet;

[0050] S15, rolling the secondary sintered blank for a second time to obtain a sintered copper-steel bimetallic sheet; the rolling amount of the second rolling is 10-15% of the thickness of the copper alloy layer in the secondary sintered blank;

[0051] S2. Impregnation treatment with impregnating agent:

[0052] The liquid impregnant is GODER-1890 type impregnant

[0053] Place the sintered copper-steel bimetallic sheet in an impregnation box, evacuate the box to a vacuum value of <-25in Hg, and then inject the liquid impregnant to allow the impregnant to enter the pores of the copper alloy layer;

[0054] S3, Carbonization:

[0055] The impregnated material is placed in a water bath and heated to solidify the liquid impregnant in the pores of the copper alloy layer at a temperature of 85°C for 30 minutes.

[0056] The solidified material was placed in a tubular furnace and heated to 600°C at a heating rate of 12°C / min in a nitrogen-hydrogen atmosphere and kept warm for 30 minutes to carbonize the infiltrant in the pores of the copper alloy layer to obtain a copper-steel bimetallic anti-friction plate.

[0057] Embodiment 2:

[0058] The preparation method of the copper-steel bimetallic anti-friction plate comprises the following steps:

[0059] S1. Preparation of sintered copper-steel bimetallic sheet:

[0060] Prepare steel plates and copper alloy powder, wherein the copper alloy powder is CuCn6Zn3Pb6 powder, and the steel plates are low-carbon steel plates No. 15 steel with a thickness of 2.5 mm.

[0061] S11, spreading the copper alloy powder on the surface of the base steel plate;

[0062] S12, placing in a sintering furnace under a protective atmosphere for the first sintering, the sintering temperature is 820°C, and the temperature is kept for 30 minutes; cooling in the furnace to obtain a primary sintered blank;

[0063] S13, rolling the primary sintered billet for the first time to obtain a primary rolled billet; the purpose of the first rolling is to increase the density of the surface layer, and the rolling amount is 40% of the thickness of the copper alloy layer in the primary sintered billet;

[0064] S14, placing the first rolled billet in a sintering furnace for a second sintering, the sintering temperature is controlled at 830° C., the duration is 20 min, and then cooling with the furnace to obtain a second sintered billet;

[0065] S15, rolling the secondary sintered blank for a second time to obtain a sintered copper-steel bimetallic sheet; the rolling amount of the second rolling is 15% of the thickness of the copper alloy layer in the secondary sintered blank;

[0066] S2. Impregnation treatment: The liquid impregnating agent is Permaseal C-2005 impregnating agent.

[0067] The sintered copper-steel bimetallic sheet is immersed in the liquid infiltrant for 10 minutes to allow the infiltrant to enter the pores of the copper alloy layer;

[0068] S3. Carbonization: Put the infiltrated material into a tubular furnace and slowly heat it in a nitrogen and hydrogen atmosphere. When it is heated to 130°C, the liquid infiltrant in the pores is solidified. Then the temperature is continued to rise to 300°C at a rate of 11°C / min. The temperature is kept for 30 minutes to carbonize the infiltrant in the pores of the copper alloy layer to obtain a copper-steel bimetallic anti-friction plate.

[0069] The microstructure of the copper-steel bimetallic anti-friction plate prepared in Example 2 was observed using a Zeiss sigma300 field emission scanning electron microscope and an energy dispersive spectrometer for component analysis. Before the observation, the material was degreased in accordance with the national standard GB / T 8643-2021 to extract the lubricating oil in the pores of the material; the electron microscope scanning image is shown in FIG. Figure 1 As shown, the carbon component (red part) analyzed by the energy spectrometer is distributed as follows Figure 2 As shown, the copper component (blue part) is distributed as Figure 3 As shown, Figure 3 The lower black area is low carbon steel. Figure 1 and Figure 2 By comparison, it can be seen that the carbon component (red part) is distributed in the pores of the copper alloy layer of the copper-steel bimetallic anti-friction plate. In addition, through scanning electron microscopy observation, the depth of carbide filling in the pores is ≥0.1mm.

[0070] Test Example 1:

[0071] Since the copper alloy layer in the copper-steel bimetallic anti-friction plate is relatively thin, directly detecting the residual carbon content in the plate may result in large errors. Therefore, this application adopts a powder metallurgy process to prepare a carburized test block. CuCn6Zn3Pb6 powder is used to press a copper-based disc sample with a diameter of 36 mm and a pressing density of 7.80-7.95 g / cm 3 , and then the same infiltration treatment and carbonization process were performed as the sintered copper-steel bimetallic plates of Examples 1 and 2. Four carbonized test blocks were prepared for each example. The samples of Example 1 were S1-1 to S1-4, and the samples of Example 2 were S2-1 to S2-4.

[0072] The test blocks prepared in each step are weighed. The weight is weighed before the infiltration treatment with the infiltrant, and its weight is calculated as the sintering weight; after the infiltration treatment with the infiltrant, the product is weighed, and the difference between the weight and the sintering weight is calculated as the infiltration amount; the product after carbonization is weighed, and the difference between the weight and the sintering weight is calculated as the carbonization amount. The details are shown in Table 1:

[0073] Table 1 Carbonization amount of Example 1-2

[0074] Group Sintered weight (g) Impregnation amount (g) Carbonization amount (g) S1-1 26.55 0.91 0.09 S1-2 26.68 0.9 0.11 S1-3 26.52 0.89 0.10 S1-4 26.73 0.91 0.10 S2-1 26.58 0.72 0.42 S2-2 26.73 0.7 0.42 S2-3 26.61 0.71 0.45 S2-4 26.56 0.71 0.44

[0075] It can be seen from Table 1 that the average carbonization amount in Example 1 of the present application is 0.10g, and the average carbonization amount in Example 2 is 0.43g. The carbonization temperature of Example 1 is 600°C, which is significantly higher than 300°C in Example 2, indicating that the temperature of the carbonization process affects the carbonization amount. High temperature will cause the carbon after carbonization of the impregnant in Example 1 to form more free activated carbon at high temperature, and the amount of carbon left in the pores of the material will become less.

[0076] Embodiment 3:

[0077] The preparation method of the copper-steel bimetallic anti-friction plate is the same as that of Example 1, except that the copper alloy powder in this example is CuSn10Pb10 powder.

[0078] The plate of Example 3 was tested in the same manner as in the above-mentioned Test Example 1, wherein the copper alloy layer was CuSn10Pb10, the final average carbonization amount was 0.11 g, and the proportion of carbon in the copper alloy was 0.41 wt%.

[0079] Comparative Example 1:

[0080] The sintered copper-steel bimetallic sheet material prepared in step S1 of Example 1 is used.

[0081] Comparative Example 2:

[0082] The sintered copper-steel bimetallic plate is prepared by step S1 of Example 1, except that the copper alloy powder is CuSn10Pb10 powder.

[0083] Comparative Example 3:

[0084] Commercially available Cu60 copper-plated graphite powder was selected, i.e., the copper content was 60wt% and the graphite content was 40wt%; the sintered copper-steel bimetallic sheet was prepared by adopting step S1 in Example 1, except that the copper alloy powder was a mixture of 99% CuSn10Pb10 powder and 1% Cu60 copper-plated graphite powder.

[0085] Test Example 2:

[0086] Tribological performance test:

[0087] HDM-200 friction and wear tester is used. The wear part rotates, the sample is placed at rest and a positive upward pressure is applied to the lower end of the sample to form sliding friction between the sample and the wear part. L-AN 32 lubricating oil is selected and placed on the test base. The friction surface of the wear part is a torus with an inner diameter of 22mm and an outer diameter of 30mm. Four 2mm wide oil grooves are evenly distributed on the torus. The surface of the sample is flat-ground Ra0.4-Ra0.8. The friction and wear performance of the sample is tested. The initial load is 800N, the loading amplitude is 400N / 10min, and the test is stopped when the oil temperature exceeds 120℃ or the friction torque exceeds 5NM. Since the friction and wear test is generally highly dispersed, 4 repeated tests are performed, and the test results are averaged, retaining three significant figures.

[0088] The friction and wear test results of Examples 1-2 and Comparative Examples 1-2 are shown in Table 2, wherein S1-1 to S1-3 are the test results of Example 1, S2-1 to S2-3 are the test results of Example 2, D1-1 to D1-3 are the test results of Comparative Example 1, and D2-1 to D2-3 are the test results of Comparative Example 2.

[0089] Table 2 Friction and wear test results of the plates in Examples 1-2 and Comparative Examples 1-2

[0090]

[0091] By comparing the friction and wear test results of Example 1 and Example 2 in combination with Table 1, it can be found that the more carbon content in the pores of the copper alloy layer, the smaller the friction coefficient and the longer the test time.

[0092] In comparative examples 1-2, the corresponding lead contents of CuCn6Zn3Pb6 and CuSn10Pb10 are 4%-8% and 7%-10% respectively. The higher the lead content, the smaller the friction coefficient and the longer the test time.

[0093] The lead content in the sintered copper-steel bimetallic sheet in Example 1 is 4%-8%, and the lead content in the sintered copper-steel bimetallic sheet in Comparative Example 2 is 7%-10%. By comparing Example 1 and Comparative Example 2, it can be found that the lead content in Example 1 is relatively small, but after the infiltration of the impregnant and carbonization, the friction coefficient of the sheet is lower than that of Comparative Example 2. This shows that to achieve the same friction coefficient, the lead content in the copper-steel bimetallic sheet can be reduced through the carbonization process, thereby reducing the impact on the human body.

[0094] By comparing Example 1 with Comparative Example 1, it can be found that since the pores in the copper alloy layer of Example 1 are filled with carburized substances, the friction performance of the material is significantly improved.

[0095] Test Example 3:

[0096] Mechanical properties testing:

[0097] The Brinell hardness test was selected, i.e., GB / T 231.1-2018 “Brinell hardness test for metallic materials Part 1: Test method”, and the copper alloy layer in the plates of Example 3, Comparative Example 2, and Comparative Example 3 was tested respectively. The results are shown in Table 3.

[0098] Table 3 Hardness test results of copper alloy layer of Example 3 and Comparative Examples 2-3

[0099]

[0100] As can be seen from Table 3, in Comparative Example 2, CuSn10Pb10 is used as the copper alloy layer, and its average hardness is 80.32HB. After adding 1% copper-plated graphite in Comparative Example 3, the hardness value of the plate becomes smaller. The main reason is that the copper-plated graphite will reduce the density of the copper alloy layer, and the copper-plated graphite has segregation; during the secondary rolling, the copper alloy layer undergoes plastic deformation, and the graphite in the pores will also deform and split the matrix, which will affect the interface quality and mechanical properties to a certain extent.

[0101] The copper alloy layer in Example 3 of the present application is CuSn10Pb10, but the hardness of the plate is significantly improved. This is because after the secondary rolling process, the infiltrant penetrates into the pores of the copper alloy layer of the sintered copper-steel bimetallic plate, and then carbonizes, and the carbonization does not affect the rolling process, and the carbon formed after carbonization remains in the pores, that is, fills in the pores to enhance the hardness of the plate and improve the mechanical properties of the plate.

[0102] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to the implementation cases and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the implementation cases herein, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A copper-steel bimetallic anti-friction sheet, comprising a substrate and a copper alloy layer, characterized in that: The substrate is an iron-based material, and the copper alloy layer is a copper alloy sintered material; the microstructure of the copper alloy layer has pores, and the pores are filled with carbides, which are solid products after the infiltration agent is infiltrated and decomposed at high temperature.

2. The copper-steel bimetallic anti-friction sheet material according to claim 1 is characterized in that: The impregnating agent is a polymer compound or a mixture, and the depth of the carbonized material filled in the pores is ≥0.1 mm.

3. The method for preparing the copper-steel bimetallic anti-friction sheet material according to claim 1 or 2, characterized in that: The following steps are involved: S1. preparing a sintered copper-steel bimetallic sheet; S2, infiltration treatment: infiltrating an infiltrant into the pores of the copper alloy layer in the sintered copper-steel bimetallic plate, wherein the infiltrant is a polymer compound or a mixture; S3. Carbonization: Heating to the carbonization temperature to carbonize the infiltrant in the pores of the copper alloy layer to obtain the copper-steel bimetallic anti-friction plate.

4. The preparation method according to claim 3, characterized in that: The preparation steps of the sintered copper-steel bimetallic sheet include: S11, spreading the copper alloy powder on the surface of the base steel plate; S12, performing the first sintering in a protective atmosphere; S13, performing a first rolling on the green body after the first sintering; S14, placing the green body after the first rolling in a sintering furnace for a second sintering; S15, rolling the blank after the second sintering for the second time to obtain a plate blank; that is, a sintered copper-steel bimetallic plate is obtained.

5. The preparation method according to claim 4, characterized in that: The base steel plate is a low-carbon steel plate; after the second rolling, a leveling machine is used for leveling.

6. The preparation method according to claim 3, characterized in that: The penetration depth of the infiltrant into the pores of the copper alloy layer is ≥0.1 mm.

7. The preparation method according to claim 3, characterized in that: The infiltrant is a liquid infiltrant; the sintered copper-steel bimetallic sheet is placed in an infiltration box, vacuumed, and then the liquid infiltrant is injected to allow the infiltrant to enter the pores of the copper alloy layer; or the sintered copper-steel bimetallic sheet is placed in the liquid infiltrant and soaked for 3-60 minutes to allow the infiltrant to enter the pores of the copper alloy layer.

8. The preparation method according to claim 3, characterized in that: The heating to the carbonization temperature means first heating to 70°C-150°C in a water bath, air or protective atmosphere for curing, and then raising the temperature to the carbonization temperature to carbonize the impregnant; wherein the carbonization temperature is 300°C-600°C, and the heating rate during the heating process is ≤12°C / min.

9. Application of the copper-steel bimetallic anti-friction sheet material as claimed in claim 1 or 2, characterized in that: The copper-steel bimetallic anti-friction plate is used for preparing mechanical parts, and the mechanical parts include rolled shaft sleeves, vane pump oil distribution plates, plunger pump oil distribution plates or gear pump side plates.

Citation Information

Patent Citations

  • Powder-coating machine for duplex metal compound material

    CN101327476B

  • Antifriction copper-based bimetallic bearing material and preparation method thereof

    CN106756214A