Gas atomization nozzle and preparation method of copper alloy powder
By using a zirconia-coated corundum precast crucible and an optimized atomizing nozzle, the problems of high oxygen content, uneven sphericity, and non-uniform particle size in copper alloy powder under non-vacuum conditions were solved, enabling efficient and continuous production of copper alloy powder and meeting the requirements of high-performance materials.
Patent Information
- Application Number
- CN202410997099.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
When preparing copper alloy powder under non-vacuum conditions, there are problems such as high oxygen content, uneven sphericity and particle size distribution, and easy clogging of nozzles, which makes it difficult to meet the requirements of high-performance materials.
The copper alloy melt is smelted using a zirconia-coated corundum precast crucible, combined with a specially designed atomizing nozzle, including optimized angles and distances of the liquid inlet channel and the first and second gas outlet channels. Inert gas protection is used, and the intermediate ladle is ceramic filtered and electromagnetic induction heated to ensure the purity and atomization effect of the copper alloy melt.
This technology enables continuous production of copper alloy powder with low oxygen content, high sphericity, and uniform particle size distribution under non-vacuum conditions, avoiding nozzle clogging and improving production efficiency and powder quality.
Smart Images

Figure CN118905230A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an aerosol nozzle and a method for preparing copper alloy powder, belonging to the technical field of alloy powder preparation. Background Art
[0002] Gas atomization powder making is a process in which liquid metal or alloy is broken into fine droplets by high-speed airflow, and then these droplets are rapidly solidified in flight to form powder. This powder making technology is widely used in powder metallurgy, 3D printing, surface coating and catalyst preparation. Gas atomization powder making can produce powders with good sphericity, high purity and narrow particle size distribution, which are suitable for high-performance materials and applications. Gas atomization powder making can be divided into vacuum gas atomization powder making and non-vacuum gas atomization powder making according to whether a vacuum environment is required during the preparation process. Vacuum gas atomization has advantages in purity, sphericity and particle size control, but the cost is high and the operation is complicated. Non-vacuum gas atomization has advantages in cost, ease of operation and large-scale production, but it is slightly inferior in purity and sphericity.
[0003] Copper and copper alloys are widely used in the fields of electricity, electronics, energy and petrochemicals, machinery and metallurgy, aerospace, marine vessels, etc. due to their excellent electrical conductivity, thermal conductivity, ductility, corrosion resistance, non-magnetic properties and high strength. With the increasing demands of the social market for short production cycles, high environmental protection requirements, and personalized customization, it is increasingly difficult to meet the requirements for copper and copper alloy components prepared by traditional casting, rolling and extrusion methods, and 3D printing copper and copper alloy technology has emerged. In additive manufacturing, the application of copper materials is relatively late, but it has shown a rapid development trend in recent years. At present, the demand for copper alloy powder for additive manufacturing in China is increasing day by day, and existing copper alloy powder manufacturers are unable to meet the relevant needs. Therefore, the development of copper alloy materials and powder making processes for additive manufacturing has received widespread attention. The gas atomization powder making method has become the main production method of alloy powder due to the continuous improvement of atomization efficiency in recent years.
[0004] In a non-vacuum environment, high-temperature copper alloys are very likely to react with oxygen in the air, which not only reduces the purity and performance of the powder, but also affects the yield and increases production costs. In addition, copper alloy powders prepared under non-vacuum conditions are often difficult to achieve the required sphericity and uniform particle size distribution. At the same time, the high thermal conductivity of copper alloys causes the metal solution to cool rapidly during the atomization process, which easily causes nozzle clogging and reduces production efficiency. For this reason, it is urgent to develop a new production method to continuously produce copper alloy powders with low oxygen content, no impurities, high sphericity and uniform particle size distribution under a non-vacuum environment. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides an aerosol nozzle and a method for preparing copper alloy powder. The produced copper alloy powder has low oxygen and nitrogen content and non-metallic inclusion content, and the powder morphology meets production requirements.
[0006] The technical solution of the present invention to solve the above technical problems is as follows:
[0007] An aerosol nozzle comprises: a liquid inlet channel, which is arranged at the axial position of an upper spray plate; an air inlet channel, which is located on the side wall of a lower spray plate; a chamber, which is formed by connecting the upper spray plate and the lower spray plate; a first air outlet channel, which is formed by extending obliquely from the inner wall of the lower spray plate toward the liquid inlet channel; and a second air outlet channel, which is arranged on the inner wall of the lower spray plate.
[0008] Preferably, the central jet line of the first air outlet channel and the outer wall extension line of the liquid inlet channel intersect at point A, the central jet line of the second air outlet channel and the outer wall extension line of the liquid inlet channel intersect at point B, and the calculation formula of the distance H between point A and point B is:
[0009]
[0010] Where l1 is the center distance of the first outlet channel, l2 is the center distance of the second outlet channel, is the diameter of the liquid inlet channel, α is the angle between the central jet line of the first air outlet channel and the extension line of the outer wall of the liquid inlet channel, β is the angle between the central jet line of the second air outlet channel and the extension line of the outer wall of the liquid inlet channel, and H is the distance between the intersection point A of the central jet line of the first air outlet channel and the extension line of the outer wall of the liquid inlet channel and the intersection point B of the central jet line of the second air outlet channel and the extension line of the outer wall of the liquid inlet channel.
[0011] Preferably, the center distance l2 is 30 to 40 mm, and the diameter is 14 to 20 mm, the center distance l1 and the diameter The difference is 1-5 mm, the angle α is 15°-25°, and the angle β is 4°-8°.
[0012] The present invention also provides a method for preparing copper alloy powder, using the atomizing nozzle described in the above scheme, comprising the following steps:
[0013] S1 Raw material preparation: Take metal raw materials with a purity of 99.9%, clean their surfaces to ensure that there are no oxide impurities and dust on the surface of the raw materials, and weigh the treated raw materials;
[0014] S2 Tundish installation: First, clean the surface of the tundish and the guide eye, and apply a special adhesive that is resistant to high temperature and chemical corrosion on the inner wall of the tundish and the contact surface of the guide eye. Place the guide eye accurately under the tundish, vertically without deviation, and apply a certain pressure to ensure that the adhesive is evenly distributed and fully in contact. Place the assembled leak bag just above the nozzle of the atomization chamber, place the tundish bonded with the guide eye by the adhesive in the graphite heating body, and ensure that the guide eye is lowered to the bottom of the graphite heating body, and the tundish does not shake. Install a refractory insulation board made of mullite insulation material on the outside and bottom of the graphite heating body, and install an electromagnetic induction coil on the outside of the refractory insulation board;
[0015] S3 Raw material smelting: In the present invention, double smelting crucibles are used for smelting, and the smelting crucibles are prefabricated corundum crucibles coated with zirconium oxide, and each of the smelting crucibles is provided with an alumina sealing cover plate with exhaust holes. The prepared raw materials are respectively loaded into the two smelting crucibles, and the sealing covers are covered. Then, inert gas is introduced into the two smelting crucibles through the exhaust holes of the sealing covers to replace the air in the smelting crucibles, and then the electromagnetic induction heater is turned on for heating until the metal material in the smelting crucible is completely melted;
[0016] S4 Atomization preparation: 5 to 10 minutes before atomization, turn on the atomizing gas heater to heat the inert atomizing gas; 2 to 3 minutes before the temperature reaches the atomizing pouring temperature, open the nozzle air intake, fill the atomizing chamber with high-temperature inert gas at a pressure of 3 to 5 MPa, turn on the fan, open the exhaust valve, and maintain for 2 minutes, so that the oxygen content in the atomizing chamber The oxygen content detector shows that the oxygen content drops below 0.1%;
[0017] S5 pouring and atomization: pouring the copper alloy melt into the tundish, the copper alloy melt flows into the atomization chamber through the tundish, adjusting the air inlet pressure of the nozzle, atomizing under the impact of high-temperature inert gas, and obtaining atomized copper alloy powder;
[0018] S6 Powder Classification: Classify the collected powder according to the particle size distribution.
[0019] Preferably, in step 2, a funnel-shaped ladle pouring gate is arranged on the top of the ladle; a ceramic filter plate is arranged below the 1 / 3 position of the bottom of the ladle, and the pore size specification of the ceramic filter plate is 50-100PPI; and the insulation layer of the ladle is a refractory insulation board made of mullite.
[0020] Preferably, in step 3, the smelting crucible is made of a prefabricated corundum crucible coated with zirconium oxide; during the smelting process, medium frequency induction heating is used to gradually increase the temperature for smelting. While the metal is smelting, the tundish is heated and kept warm by gradually increasing the temperature.
[0021] Preferably, in step 3, after the metal is completely melted, the heating power is reduced and a slag-forming agent is added to the smelting crucible.
[0022] Preferably, the pouring temperature of step 5 is 1430-1470° C., and the pouring point of the copper alloy melt is located between the inner ring edge of the funnel-shaped ladle gate and the 1 / 3 position of the inner ring edge extending outward.
[0023] Preferably, in step 5, the atomization pressure is 4 to 5 MPa.
[0024] Preferably, in step 6, the powder is classified using an integrated airflow classification device, the fan frequency is 40-50 Hz, the classification frequency is 8-10 Hz, and the particle size distribution requirements are: D10: 15-25 μm, D50: 30-40 μm, D90: 53-58 μm.
[0025] The beneficial effects of the present invention are:
[0026] In the preparation method of the copper alloy powder described in the present invention, under non-vacuum conditions, the alloy material is smelted in a corundum prefabricated crucible coated with zirconium oxide, and poured using a specially installed tundish. By using a designed atomizing nozzle, the copper alloy powder continuously produced has an oxygen content of less than 0.05%, a powder sphericity of more than 90%, and a powder particle size distribution that meets production standards.
[0027] The nozzle used in the present invention reduces the collision probability of atomized incompletely solidified powder and solidified powder, reduces the content of irregular powder, and controls the oxygen content, powder morphology and particle size distribution of copper alloy powder by controlling the diameter of the liquid inlet channel, the center distance between the first gas outlet channel and the second gas outlet channel, the angle between the central jet line of the first gas outlet channel and the extension line of the inner wall of the liquid inlet channel, and the angle between the central jet line of the second gas outlet channel and the extension line of the inner wall of the liquid inlet channel. At the same time, it avoids the powder back-spraying after atomization, resulting in bag blockage, and affecting the continuous production of copper alloy powder.
[0028] In the present invention, a zirconium oxide-coated corundum prefabricated crucible is used as a smelting crucible. Compared with a traditional corundum crucible, the zirconium oxide coating can prevent the Al2O3 component in the corundum crucible from transferring oxygen to the metal melt, resulting in the burning of alloy elements or the generation of new non-metallic impurities, thereby effectively improving the purity of the copper alloy melt. In addition, zirconium oxide is more resistant to high temperatures than aluminum oxide, which is conducive to the continuous production of copper alloy powder.
[0029] In the tundish used in the present invention, the guide leak eye, tundish body, graphite heating body, mullite refractory insulation board, electromagnetic induction coil, leak ladle gate, ceramic filter plate and other parts cooperate with each other, which greatly improves the insulation effect of the tundish, reduces the risk of clogging, realizes continuous production, and improves the atomization effect of the molten copper alloy melt, extending the service life of the tundish and the atomizing nozzle. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a cross-sectional view of the atomizing nozzle of the present invention;
[0031] Figure 2 It is a partial enlarged view of the cross-sectional view of the atomizing nozzle in the present invention;
[0032] Figure 3 The scanning electron microscope image of the powder prepared in Example 1 of the present invention;
[0033] Figure 4 It is a smelting process curve diagram in the present invention;
[0034] Figure 5 This is a powder morphology image prepared in Comparative Example 2 of the present invention;
[0035] Figure 6 This is a state diagram of the atomizing nozzle after the preparation of comparative example 5 of the present invention is completed.
[0036] In the figure, 1, liquid inlet channel; 2, air inlet channel; 3, chamber; 4, outer wall extension line of liquid inlet channel; 5, first air outlet channel; 6, second air outlet channel; 7, upper spray plate; 8, lower spray plate; 9, central spray line of first air inlet channel; 10, central spray line of second air inlet channel. DETAILED DESCRIPTION
[0037] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0039] An aerosol nozzle includes a liquid inlet channel 1, an air inlet channel 2, a chamber 3 and an air outlet channel. The liquid inlet channel 1 is arranged at the axial center of the upper spray plate 7; the air inlet channel 2 is located at the upper and lower center of the side wall of the lower spray plate 8; the chamber 3 is formed by connecting the upper spray plate 7 and the lower spray plate 8; the first air outlet channel 5 is formed by the inner wall of the lower spray plate 8 extending obliquely toward the liquid inlet channel 1; the second air outlet channel 6 is arranged on the inner wall of the lower spray plate 8, such as Figure 1 As shown;
[0040] In this example, the atomizing nozzle is provided with two groups of air outlet channels. The first air outlet channel 5 is a gap-shaped channel formed by the inner wall of the lower spray plate 8 of the atomizing nozzle obliquely extending toward the liquid inlet channel, and is formed by the upper spray plate 7 and the liquid inlet channel 1, and the second air outlet channel 6 is a rod-shaped through hole evenly distributed on the inner wall of the lower spray plate 8.
[0041] In order to reduce the collision probability between the atomized incompletely solidified powder and the solidified powder, reduce the content of the irregular powder, and thereby control the oxygen content, powder morphology and particle size distribution of the copper alloy powder, and avoid the powder back-spraying after atomization, resulting in blockage and affecting the continuous production of the copper alloy powder, the distance between the intersection A of the central jet line 9 of the first air outlet channel 5 and the outer wall extension line 4 of the liquid inlet channel 1 and the intersection B of the central jet line 10 of the second air outlet channel 6 and the outer wall extension line 4 of the liquid inlet channel 1 is limited, that is, the calculation formula of the distance between the intersection A and the intersection B is:
[0042]
[0043] Where l1 is the center distance of the first air outlet channel 5, l2 is the center distance of the second air outlet channel 6, is the diameter of the liquid inlet channel 1, α is the angle between the central jet line 9 of the first gas outlet channel 5 and the outer wall extension line 4 of the liquid inlet channel 1, β is the angle between the central jet line 10 of the second gas outlet channel 6 and the outer wall extension line 4 of the liquid inlet channel 1, H is the distance between the intersection point A of the central jet line 9 of the first gas outlet channel 5 and the outer wall extension line 4 of the liquid inlet channel 1 and the intersection point B of the central jet line 10 of the second gas outlet channel 6 and the outer wall extension line 4 of the liquid inlet channel 1, as shown in FIG. Figure 2 shown.
[0044] During the atomization process, the molten copper alloy melt enters the atomizing nozzle through the liquid inlet channel 1, and the high-temperature inert gas enters the chamber 3 through the gas inlet channel 2, forming a high pressure in the chamber 3. Under the action of high pressure, the inert gas enters the nozzle through the first gas outlet channel 5 and meets the molten copper alloy melt, thereby forming an atomization zone of the copper alloy melt. The molten copper alloy melt is impacted by the high-speed airflow in the atomization zone to form fine copper alloy melt droplets, which then solidify to form metal powder.
[0045] The angle α between the central jet line 9 of the first air outlet channel 5 and the outer wall extension line 4 of the liquid inlet channel 1 is 15°~25°. When the angle is too large, the closer the airflow is to the molten metal when it flows out of the nozzle, the greater the kinetic energy of the airflow in contact with the molten metal, but the greater the degree of flow turbulence when the airflows intersect, which will increase the resistance to the outflow of the molten metal and easily cause blockage; when the angle is too small, the distance H between the intersection A of the central jet line 9 of the first air outlet channel 5 and the outer wall extension line 4 of the liquid inlet channel 1 and the intersection B of the central jet line 10 of the second air outlet channel 6 and the outer wall extension line 4 of the liquid inlet channel 1 is too small, and the molten metal is not atomized in time, resulting in energy loss, so that the atomized powder has low sphericity and uneven particle size distribution.
[0046] After the molten copper alloy is atomized by the airflow of the first air outlet channel 5, spherical metal droplets of different diameters will be formed. Smaller droplets will solidify quickly, while larger droplets will solidify slowly. When the powder falls to a certain extent, the solidified small powder will move to the atomization area due to the influence of the airflow in the atomization chamber. In this process, the solidified small powder will adhere to the droplets that have just been atomized and have not yet solidified, and form special-shaped powder after solidification, thereby affecting the powder morphology. The second air outlet channel 6 set on the side wall of the lower spray plate 8 can form an airflow barrier below the atomization area to block the powder moving to the atomization area with the airflow in the atomization chamber. At the same time, the solidified powder is pressed down to reduce the collision probability of the solidified small powder and the unsolidified droplets, thereby avoiding the formation of special-shaped powder.
[0047] The angle β between the central jet line 10 of the second air outlet channel 6 and the outer wall extension line 4 of the liquid inlet channel 1 is set to 4°~8°. When the angle is too large, the airflow of the second air outlet channel 6 will disturb the airflow of the first air outlet channel and reduce the atomization efficiency; when the angle is too small, the distance H between the intersection A of the central jet line 9 of the first air outlet channel 5 and the outer wall extension line 4 of the liquid inlet channel 1 and the intersection B of the central jet line 10 of the second air outlet channel 6 and the outer wall extension line 4 of the liquid inlet channel 1 is too large, which weakens the ability to suppress subdivision returning with the airflow in the atomization chamber, and is not conducive to the formation of good powder morphology.
[0048] In addition, the center distance l2 of the second air outlet channel 6 is 30-40 mm. The smaller the center distance l2 of the second air outlet channel 6, the greater the air flow rate in the atomization zone, and the more difficult it is for the atomized powder to approach the atomization zone, thereby reducing the probability of contact between the unsolidified atomized powder and the solidified atomized powder, thereby reducing the content of irregular powder; when the center distance l2 of the second air outlet channel 6 is larger, the blank space between the two air flow channels is larger, and the air flow ejected from the second air outlet channel 6 will instead press the unsolidified powder sharply between the first air outlet channel 5 and the second air outlet channel 6, thereby bonding to the inner wall of the lower spray plate and the blank space between the first air outlet channel 5 and the second air outlet channel 6, affecting the continuity of production.
[0049] A method for preparing copper alloy powder by non-vacuum gas atomization for casting and smelting, the method comprising the following steps:
[0050] S1, raw material assembly: take metal raw materials with a purity of 99.9%, clean their surfaces to ensure that there are no oxide impurities and dust on the surface of the raw materials, and weigh the treated raw materials;
[0051] S2, installation of tundish: During the assembly of the tundish, firstly, the inside of the tundish body and the surface of the guide eye are thoroughly cleaned to remove oxide impurities, dust and other dirt; then, a layer of special adhesive that can withstand high temperature and chemical corrosion is applied to the bottom of the tundish body and the top of the guide eye to ensure that the adhesive is evenly covered; then, the part of the guide eye coated with the adhesive is accurately placed on the part of the tundish coated with the adhesive, keeping it vertical and not skewed, and applying appropriate pressure to ensure that the adhesive is evenly distributed and fully fits the contact surface; then, the bonded tundish body is placed in the graphite heating body, ensuring that the guide eye is lowered to the bottom of the graphite heating body, and the tundish is fixed and stable without shaking; then, A layer of refractory insulation board made of mullite insulation material is installed on the outside of the graphite heating body, and an electromagnetic induction coil is fixed on the outside of the insulation board to heat the tundish; then, a layer of mullite refractory insulation material is laid on the bottom of the tundish shell, and the assembled tundish is securely placed in the shell; then, a funnel-shaped ladle gate is installed on the upper part of the tundish, and a ceramic filter plate with a pore size of 50 to 100 PPI is fixed inside the tundish using an adhesive that can withstand high temperatures and chemical corrosion, located below 1 / 3 of the bottom of the tundish; finally, the refractory insulation cover is covered, and the entire installed tundish is placed directly above the atomizing nozzle of the atomizing chamber, so that the guide eye of the tundish is connected to the atomizing nozzle.
[0052] Due to the excellent thermal conductivity of copper alloys, and in a non-vacuum environment, the tundish is not continuously heated and dissipates heat quickly. Therefore, when the copper alloy metal solution is poured into the tundish, the metal solution will solidify rapidly under a large temperature drop, blocking the guide eye, causing the pouring system to be blocked. In order to solve this problem, the tundish adopts electromagnetic induction heating technology. Although the induction coil can heat and melt the metal, the pouring temperature of the copper alloy metal solution is as high as 1430-1470°C, and the insulation temperature of the tundish needs to be maintained at 1200-1300°C. The electromagnetic induction heating coil is made of copper, and its melting point is 1083.4°C, which will cause the induction coil to deform rapidly or even melt at high temperatures. Adding a mullite insulation board between the electromagnetic induction coil and the graphite heating body can provide thermal insulation protection for the electromagnetic induction coil. At the same time, mullite is a positive thermal expansion material, which can make the graphite heating body fit closely with the tundish during the heating process, thereby improving the heating efficiency of the electromagnetic induction coil and increasing the insulation effect of the tundish. Similarly, since the bottom of the tundish is directly connected to the atomization chamber, the atomization nozzle, as a key component of the gas atomization process, is very likely to expand and contract under the influence of temperature changes, causing its first gas outlet channel 5 to deform, thereby affecting the atomization effect. Therefore, a mullite insulation plate is also provided at the bottom of the tundish and above the nozzle to protect the nozzle from high temperature and ensure the smooth progress of the atomization process.
[0053] In the pouring process of non-vacuum air atomization powder making, the liquid storage pouring method is adopted, that is, during the pouring atomization process, the tundish is always covered with copper alloy melt. When the refractory insulation cover of the tundish is opened for pouring, air will enter the tundish together with the copper alloy melt under the action of suction, and react with the metal solution under high temperature conditions to generate metal oxide impurities, thereby increasing the oxygen content of the powder. Fixing the ceramic filter below the 1 / 3 position of the bottom of the tundish can effectively filter out metal oxide impurities, and at the same time filter out the slag-forming agent and other non-metallic impurities added during the refining process that have not been cleaned up, thereby improving the purity of the final product.
[0054] S3, raw material smelting: In the present invention, two prefabricated corundum crucibles coated with zirconium oxide are used for smelting. Before adding the metal raw materials, the inside of the smelting crucible is first cleaned to ensure that there are no impurities and dust. Subsequently, the configured raw materials are respectively loaded into two smelting crucibles, and covered with a sealing cover plate with exhaust holes; an inert gas is introduced into the two smelting crucibles through the exhaust holes of the sealing cover plate to replace the air in the smelting crucible; the electromagnetic induction heater is turned on, and the heating power is first adjusted to 40±2kw, and kept warm for 15 minutes, and then the heating power is increased to 80±2kw, and kept warm for 15 minutes, and then the heating power is increased to 120±2kw, and kept warm again for 15 minutes, and then the heating power is increased to 160±2 kw, continue to keep warm for 15 minutes, and finally, increase the heating power to 180±2kw until the metal material in the melting crucible is completely melted; after the copper alloy metal solution is completely cleared, reduce the heating power to 100kw, remove the sealing cover, and immediately add slag-forming agent to the melting crucible, and keep the copper alloy solution with a superheat of 100-150℃ for 20 minutes; then, increase the heating power to 180±2kw until the surface film of the copper alloy metal solution breaks, and quickly remove a large amount of slag-forming agent floating on the surface of the melt, such as Figure 4 As shown; while the raw materials are being melted, the tundish is preheated and kept warm by medium frequency induction heating. The temperature is gradually increased. First, the heating power is adjusted to 6±0.5kw and kept warm for 15 minutes. Then, the heating power is increased to 8±0.5kw and kept warm for 15 minutes. Then, the heating power is increased to 10±0.5kw and kept warm for another 15 minutes. After that, the heating power is increased to 12±0.5kw and kept warm for 15 minutes. Finally, the heating power is increased to 14±0.5kw, and the melting crucible is heated to 1200-1300℃ and kept warm.
[0055] During the induction melting process, Al2O3, the main component of the corundum crucible, is easily decomposed at high temperatures and transfers oxygen to the metal melt, which not only causes the oxygen content in the alloy to exceed the standard, but also may cause O to react with active elements in the alloy, causing the alloy elements to burn out and produce new non-metallic inclusions. These newly generated inclusions will accelerate the erosion of the melting crucible. In contrast, ZrO2 has higher thermodynamic stability, and the oxidation potential of ZrO2 is much smaller than that of Al2O3, which makes ZrO2 have weak oxygen transfer ability, thereby reducing the probability of the molten copper alloy reacting with oxygen, thereby improving the purity of the copper alloy powder finally produced. In addition, ZrO2 has high high temperature resistance, which is conducive to the continuous production of copper alloy powder.
[0056] In the copper alloy smelting process, a lower power current is used to supply electricity at the initial stage so that heating can remove the gas adsorbed by the material in the melting crucible. If the temperature rises too quickly and the inert gas filling rate is not enough to replace the air in the melting crucible in time, the copper alloy may react with the oxygen in the air, resulting in an increase in the oxygen content in the product. Subsequently, the power is gradually increased to increase the temperature, so that the chemical reactions that may occur during the smelting process can be observed and controlled to ensure the purity and quality of the smelting process. In addition, the gradual heating strategy also helps to reduce energy consumption during the smelting process, and the insulation at each temperature gradient also helps to reduce energy waste.
[0057] Since the tundish body and the guide eye, as well as the tundish and the ceramic filter are bonded together by a binder that is resistant to high temperatures and chemical corrosion, gradually increasing the temperature can reduce the internal thermal stress of the binder caused by rapid temperature changes, ensure that the binder works stably at gradually increasing temperatures, avoid bonding failure caused by sudden temperature changes, and thus reduce the risk of cracks in the bonding parts of the tundish and the guide eye. At the same time, it is coordinated with the metal melting rate to avoid the need to maintain the temperature for a long time after reaching the specified temperature due to excessive heating to wait for the copper alloy in the melting crucible to melt, resulting in unnecessary energy waste.
[0058] S4, atomization preparation: 5 to 10 minutes before atomization, turn on the atomizing gas heater to heat the inert atomizing gas; 2 to 3 minutes before the temperature of the molten metal after slagging approaches 1430 to 1470°C, start the atomizing nozzle air inlet valve, fill the atomizing chamber with high-temperature inert gas, maintain the air pressure of the atomizing nozzle at 3 to 5 MPa, and at the same time, turn on the fan and exhaust valve for 2 to 4 minutes to reduce the oxygen content in the atomizing chamber to below 0.1%;
[0059] S5, pouring and atomization: before pouring, first adjust the air inlet pressure of the atomizing nozzle to 3-7MPa, and start introducing inert gas; then, move the melting crucible on one side to the front of the tundish, open the sealing cover of the tundish, tilt the melting crucible, ensure that the pouring point of the copper alloy melt is between the inner ring edge of the funnel-shaped ladle gate of the tundish and the 1 / 3 position of the inner ring edge extending outward, start pouring and atomization, and closely monitor the remaining amount of the copper alloy melt, and move the melting crucible on the other side to the front of the tundish in time to realize a continuous atomization powder making process.
[0060] It should be noted that during the pouring process, the pouring point of the molten copper alloy should fall between the inner ring edge of the tundish ladle gate and the position 1 / 3 of the inner ring edge extending outward. Since the material of the tundish ladle gate is ceramic refractory, its strength is limited, and the impact force of the molten copper alloy is large at the beginning of pouring. Under the multiple impacts of the high-temperature copper alloy melt, the outside of the ladle gate is extremely prone to cracking, thereby reducing the service life of the ladle gate; in addition, under the large impact force of the copper alloy melt, the copper alloy melt impacts the ladle gate, which easily causes the copper alloy melt to splash violently. If the pouring point of the copper alloy melt is too high, it will cause the copper alloy melt to splash out of the diameter range of the ladle gate, thereby causing a safety accident.
[0061] S6, powder classification: in an inert gas environment, use an integrated airflow classification device with a fan frequency of 40 to 50 Hz and a classification frequency of 8 to 10 Hz. Measure the particle size distribution of the cooled copper alloy metal powder according to the laser diffraction method of GB / T 19077. Determine the particle size of the cooled copper alloy metal powder according to the dry sieving method of GB / T 1480. The particle size distribution requirements are: D10: 15 to 25 μm, D50: 30 to 40 μm, and D90: 53 to 58 μm.
[0062] In addition, the inert gas used in the present invention is a gas that does not react with the alloy in the technical solution, preferably argon, and other gases that meet the above conditions may also be used.
[0063] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0064] Example 1
[0065] S1, raw material assembly: clean the surface of each raw material that meets the national standard requirements to ensure that there is no oxide impurities and dust on the surface of the raw material, and weigh the processed raw materials; the weight percentage of each raw material is: nickel 30%, manganese 0.9%, iron 1.0%, niobium 0.6%, and copper is the balance;
[0066] S2, Tundish installation: Correctly install the tundish and add a ceramic filter with a pore density of 50PPI.
[0067] S3, raw material smelting: load the prepared charge into two melting crucibles respectively, cover with insulation board, input inert gas to replace the air in the melting crucible, set the power of medium frequency furnace, and gradually increase the melting power from 40kw to 180kw. At the same time, turn on the induction heating of the tundish, set the medium frequency heating power, and gradually increase the melting power from 6kw to 14kw, heat the tundish to 1200℃ and keep it warm; the melting crucible is charged with copper as the basis, and iron, nickel, niobium, etc. are placed in the middle of the melting crucible. Manganese can be added for the second time after the alloy is melted. After the alloy is melted, reduce the power of medium frequency furnace to 100kw, cover the surface of alloy liquid with slag-forming agent, and keep warm for refining. After refining is completed, increase the power of medium frequency furnace to 180kw to increase the temperature of the alloy, quickly remove the slag on the surface of the alloy melt at 1380±20℃, and maintain the power of 180kw for heating;
[0068] S4, atomization preparation: 5 minutes before atomization, turn on the atomization gas heater to heat the inert atomization gas; 3 minutes before the temperature reaches the atomization pouring temperature, open the nozzle air intake, fill the atomization chamber with high-temperature inert gas at a pressure of 3MPa, turn on the fan, open the exhaust valve, maintain for 2 minutes, and the oxygen content detector in the atomization chamber shows that the oxygen content is 0.08%;
[0069] S5, pouring and atomization: use a hydraulic device to move one side of the melting crucible to a limited position, and pour the 1450°C alloy melt in the melting crucible into the tundish. When the current melting crucible is pouring, the melting crucible on the other side is heated to the pouring temperature and prepared to continue pouring, so as to maintain the continuity of the pouring of the copper alloy melt. The copper alloy melt flows into the atomization chamber through the tundish, and is atomized under the impact of the high-temperature inert gas, and the alloy melt is quickly broken into spherical droplets, which are quickly cooled to form powder under the cooling effect of the atomizing gas and the surface tension of the copper alloy melt droplets; the angle α between the central jet line 9 of the first gas outlet channel 5 of the atomizing nozzle and the outer wall extension line 4 of the liquid inlet channel 1 is 15°, the angle β between the central jet line 10 of the second gas outlet channel 6 and the outer wall extension line 4 of the liquid inlet channel 1 is 8°, the center distance l2 of the second gas outlet channel 6 is 30 mm, and the diameter of the liquid inlet channel The diameter is 18mm, and the atomization pressure is 4MPa;
[0070] S6, powder classification: In an inert gas environment, an integrated airflow classification device was used, with a fan frequency of 40 Hz and a classification frequency of 8 Hz. The particle size distribution of the cooled copper alloy metal powder was measured according to the laser diffraction method of GB / T 19077. The particle size of the cooled copper alloy metal powder was measured according to the dry sieving method of GB / T 1480. The obtained particle size distribution was: D10: 21.3 μm, D50: 38.3 μm, D90: 57.3 μm, as shown in Figure 5. Figure 3 shown.
[0071] Example 2
[0072] S1, raw material assembly: clean the surface of each raw material that meets the national standard requirements to ensure that there is no oxide impurities and dust on the surface of the raw material, and weigh the processed raw materials; the weight percentage of each raw material is: nickel 30%, manganese 0.9%, iron 1.0%, niobium 0.6%, and copper is the balance;
[0073] S2, Tundish installation: Install the tundish correctly and add a ceramic filter with a pore density of 70PPI
[0074] S3, raw material smelting: Raw material smelting: Load the prepared charge into two melting crucibles respectively, cover with insulation board, input inert gas to replace the air in the melting crucible, set the power of medium frequency furnace, and gradually increase the melting power from 40kw to 180kw. At the same time, turn on the induction heating of the tundish, set the medium frequency heating power, and gradually increase the melting power from 6kw to 14kw, heat the tundish to 1200℃ and keep it warm; the melting crucible is charged with copper as the basis, and iron, nickel, niobium, etc. are placed in the middle of the melting crucible. Manganese can be added for the second time after the alloy is melted. After the alloy is melted, reduce the power of the medium frequency furnace to 100kw, cover the surface of the alloy liquid with slag-forming agent, and keep warm for refining. After the refining is completed, increase the power of the medium frequency furnace to 180kw to increase the alloy temperature, and quickly remove the slag on the surface of the alloy melt at 1380±20℃, and maintain the power of 180kw for heating;
[0075] S4, atomization preparation: 5 minutes before atomization, turn on the atomization gas heater to heat the inert atomization gas; 3 minutes before the temperature reaches the atomization pouring temperature, open the nozzle air intake, fill the atomization chamber with high-temperature inert gas at a pressure of 4MPa, turn on the fan, open the exhaust valve, maintain for 2 minutes, and the oxygen content detector in the atomization chamber shows that the oxygen content is 0.06%;
[0076] S5, pouring and atomization: use a hydraulic device to move one side of the melting crucible to a limited position, and pour the 1450°C alloy melt in the melting crucible into the tundish. When the current melting crucible is pouring, the melting crucible on the other side is heated to the pouring temperature and prepared to continue pouring, so as to maintain the continuity of the pouring of the copper alloy melt. The copper alloy melt flows into the atomization chamber through the tundish, and is atomized under the impact of the high-temperature inert gas, and the alloy melt is quickly broken into spherical droplets, which are quickly cooled to form powder under the cooling effect of the atomizing gas and the surface tension of the copper alloy melt droplets; the angle α between the central jet line 9 of the first gas outlet channel 5 and the outer wall extension line 4 of the liquid inlet channel 1 is 20°, the angle β between the central jet line 10 of the second gas outlet channel 6 and the outer wall extension line 4 of the liquid inlet channel 1 is 6°, the center distance l2 of the second gas outlet channel 6 is 35 mm, and the diameter of the liquid inlet channel The diameter is 18mm, and the atomization pressure is 4.5MPa;
[0077] S6, powder classification: In an inert gas environment, using an integrated airflow classification device, with a fan frequency of 45Hz and a classification frequency of 9Hz, the particle size distribution of the cooled copper alloy metal powder is measured according to the GB / T 19077 laser diffraction method, and the particle size of the cooled copper alloy metal powder is measured according to the GB / T 1480 dry sieving method. The particle size distribution requirements are: D10: 20.9μm, D50: 39.9μm, D90: 57.1μm. .
[0078] Example 3
[0079] S1, raw material assembly: clean the surface of each raw material that meets the national standard requirements to ensure that there is no oxide impurities and dust on the surface of the raw material, and weigh the processed raw materials; the weight percentage of each raw material is: nickel 30%, manganese 0.9%, iron 1.0%, niobium 0.6%, and copper is the balance;
[0080] S2, Tundish installation: Install the tundish correctly and add a ceramic filter with a pore density of 100PPI
[0081] S3, raw material smelting: Raw material smelting: Load the prepared charge into two melting crucibles respectively, cover with insulation board, input inert gas to replace the air in the melting crucible, set the power of medium frequency furnace, and gradually increase the melting power from 40kw to 180kw. At the same time, turn on the induction heating of the tundish, set the medium frequency heating power, and gradually increase the melting power from 6kw to 14kw, heat the tundish to 1200℃ and keep it warm; the melting crucible is charged with copper as the basis, and iron, nickel, niobium, etc. are placed in the middle of the melting crucible. Manganese can be added for the second time after the alloy is melted. After the alloy is melted, reduce the power of the medium frequency furnace to 100kw, cover the surface of the alloy liquid with slag-forming agent, and keep warm for refining. After the refining is completed, increase the power of the medium frequency furnace to 180kw to increase the alloy temperature, and quickly remove the slag on the surface of the alloy melt at 1380±20℃, and maintain the power of 180kw for heating;
[0082] S4, atomization preparation: 5 minutes before atomization, turn on the atomization gas heater to heat the inert atomization gas; 3 minutes before the temperature reaches the atomization pouring temperature, open the nozzle air intake, fill the atomization chamber with high-temperature inert gas at a pressure of 5MPa, turn on the fan, open the exhaust valve, maintain for 2 minutes, and the oxygen content detector in the atomization chamber shows that the oxygen content is 0.04%;
[0083] S5, pouring and atomization: use a hydraulic device to move one side of the melting crucible to a limited position, and pour the 1470°C alloy melt in the melting crucible into the tundish. When the current melting crucible is pouring, the melting crucible on the other side is heated to the pouring temperature and prepared to continue pouring, so as to maintain the continuity of the pouring of the copper alloy melt. The copper alloy melt flows into the atomization chamber through the tundish, and is atomized under the impact of the high-temperature inert gas, and the alloy melt is quickly broken into spherical droplets, which are quickly cooled to form powder under the cooling effect of the atomizing gas and the surface tension of the copper alloy melt droplets; the angle α between the central jet line 9 of the first gas outlet channel 5 of the atomizing nozzle and the outer wall extension line 4 of the liquid inlet channel 1 is 25°, the angle β between the central jet line 10 of the second gas outlet channel 6 and the outer wall extension line 4 of the liquid inlet channel 1 is 4°, the center distance l2 of the second gas outlet channel 6 is 40mm, and the diameter of the liquid inlet channel The diameter is 18mm, and the atomization pressure is 5MPa;
[0084] S6, powder classification: In an inert gas environment, using an integrated airflow classification device, with a fan frequency of 50Hz and a classification frequency of 10Hz, the particle size distribution of the cooled copper alloy metal powder is measured according to the laser diffraction method of GB / T 19077, and the particle size of the cooled copper alloy metal powder is measured according to the dry sieving method of GB / T 1480. The particle size distribution requirements are: D10: 18.0μm, D50: 36.8μm, D90: 56.5μm.
[0085] Comparative Example 1
[0086] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 uses a corundum prefabricated crucible to melt metal materials.
[0087] Comparative Example 2
[0088] The difference between Comparative Example 2 and Example 1 is that in Comparative Example 2, the atomizing nozzle disclosed in Patent CN 116604023 is used to gas-atomize the copper alloy melt.
[0089] Comparative Example 3
[0090] The difference between Comparative Example 3 and Example 1 is that the angle α between the central injection line 9 of the first air outlet channel 5 of the atomizing nozzle used in Comparative Example 3 and the outer wall extension line 4 of the liquid inlet channel 1 is 10°.
[0091] Comparative Example 4
[0092] The difference between Comparative Example 4 and Example 1 is that the angle β between the central injection line 10 of the second air outlet channel 6 of the atomizing nozzle used in Comparative Example 4 and the outer wall extension line 4 of the liquid inlet channel 1 is 3°.
[0093] Comparative Example 5
[0094] The difference between Comparative Example 5 and Example 1 is that the center distance l2 of the second air outlet channel 6 used in Comparative Example 5 is 45 mm.
[0095] Table 1 Test results of powders obtained in Examples and Comparative Examples
[0096]
[0097] It can be seen from Examples 1 to 3 that the copper alloy powders prepared using the atomizing nozzle and the preparation method of the present invention have oxygen contents lower than 0.05%, powder sphericity higher than 90%, and a 15-53 μm powder yield higher than 35%.
[0098] It can be seen from Comparative Example 1 and Example 1 that when a corundum precast crucible is used to melt metal, the oxygen content in the powder is higher than 0.05%. Al2O3, the main component of the corundum precast crucible, transfers oxygen to the metal melt under high temperature conditions, resulting in excessive oxygen content in the alloy.
[0099] It can be seen from Comparative Example 2 and Example 1 that when the atomizing nozzle disclosed in Patent CN 110899713 is used for atomization, the sphericity of the powder is less than 90%, and the yield of 15-53 μm powder is less than 35%. Figure 5 As shown in the figure, since the angle of the first gas outlet channel is too small and the angle of the second gas outlet channel is too large, the distance between the intersection point A of the central jet line of the first gas outlet channel and the extension line of the outer wall of the liquid inlet channel and the intersection point B of the central jet line of the second gas outlet channel and the extension line of the outer wall of the liquid inlet channel is not suitable, which reduces the sphericity of the powder and the powder yield is poor.
[0100] It can be seen from Comparative Example 3 and Example 1 that if the angle α between the central jet line of the first air outlet channel of the atomizing nozzle and the extension line of the outer wall of the liquid inlet channel is too small, the distance H between the intersection A of the central jet line of the first air outlet channel and the extension line of the outer wall of the liquid inlet channel and the intersection B of the central jet line of the second air outlet channel and the extension line of the outer wall of the liquid inlet channel is too short, resulting in untimely atomization, resulting in low sphericity of the atomized powder, uneven particle size distribution, and even blockage.
[0101] It can be seen from Comparative Example 4 and Example 1 that since the angle β between the central jet line of the second air outlet channel and the extension line of the outer wall of the liquid inlet channel is too small, the distance H between the intersection A of the central jet line of the first air outlet channel and the extension line of the outer wall of the liquid inlet channel and the intersection B of the central jet line of the second air outlet channel and the extension line of the outer wall of the liquid inlet channel is too large, which weakens the ability to suppress subdivision returning with the airflow in the atomization chamber, and is not conducive to the formation of good powder morphology.
[0102] It can be seen from the comparative example 5 and the embodiment 1 that when the center distance l2 of the second air outlet channel is too large, the airflow ejected from the second air outlet channel will instead press the unsolidified powder sharply to the space between the first air outlet channel and the second air outlet channel, and adhere to the blank space between the first air outlet channel and the second air outlet channel on the inner wall of the lower spray plate. Figure 6 shown.
[0103] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0104] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. An aerosol nozzle, characterized in that: include: A liquid inlet channel (1), wherein the liquid inlet channel (1) is arranged at the axial center position of the upper spray plate (7); An air inlet channel (2), wherein the air inlet channel (2) is located on a side wall of the lower spray plate (8); A chamber (3), wherein the chamber is formed by connecting an upper spray plate (7) and a lower spray plate (8); A first air outlet channel (5), the first air outlet channel (5) being formed by the inner wall of the lower spray plate (8) extending obliquely toward the liquid inlet channel (1); A second air outlet channel (6), wherein the second air outlet channel (6) is arranged on the inner wall of the lower spray plate (8).
2. An aerosol nozzle according to claim 1, characterized in that: The central jet line (9) of the first air outlet channel (5) and the outer wall extension line (4) of the liquid inlet channel (1) intersect at point A, and the central jet line (10) of the second air outlet channel (6) and the outer wall extension line (4) of the liquid inlet channel (1) intersect at point B. The calculation formula for the distance H between point A and point B is: Wherein l1 is the center distance of the first air outlet channel (5), l2 is the center distance of the second air outlet channel (6), is the diameter of the liquid inlet channel (1), α is the angle between the central jet line (9) of the first air outlet channel (5) and the outer wall extension line (4) of the liquid inlet channel (1), β is the angle between the central jet line (10) of the second air outlet channel (6) and the outer wall extension line (4) of the liquid inlet channel (1), and H is the distance between the intersection point A of the central jet line (9) of the first air outlet channel (5) and the outer wall extension line (4) of the liquid inlet channel (1) and the intersection point B of the central jet line (10) of the second air outlet channel (6) and the outer wall extension line (4) of the liquid inlet channel (1).
3. An aerosol nozzle according to claim 2, characterized in that: The center distance l2 is 30 to 40 mm, and the diameter is 14 to 20 mm, the center distance l1 and the diameter The difference is 1-5 mm, the angle α is 15°-25°, and the angle β is 4°-8°.
4. A method for preparing copper alloy powder, using the atomizing nozzle according to any one of claims 1 to 3, comprising the following steps: S1 Raw material preparation: clean the surface of the raw materials and weigh them according to the formula; S2 Tundish installation: install the guide leak at the bottom of the tundish, place the tundish in the graphite heating body, and sequentially set the insulation board and the electromagnetic induction coil outside the graphite heating body; S3 raw material smelting: put the prepared raw materials into the smelting crucible, cover it with a sealing cover with holes, replace the air in the smelting crucible, and smelt to obtain an alloy solution; S4 Atomization preparation: introduce high-temperature inert atomizing gas into the atomizing chamber to replace the air in the atomizing chamber so that the oxygen content in the atomizing chamber is less than 0.1%; S5 pouring and atomization: pouring the alloy solution that meets the pouring conditions from the melting crucible into the tundish and performing gas atomization; S6 Powder Classification: Classify the collected powder according to the particle size distribution.
5. A method for preparing copper alloy powder according to claim 4, characterized in that: In step S2, a funnel-shaped ladle pouring gate is arranged on the top of the tundish; a ceramic filter plate is arranged below the 1 / 3 position of the bottom of the tundish, and the pore size specification of the ceramic filter plate is 50-100PPI; and the insulation layer of the tundish is a refractory insulation board made of mullite.
6. A method for preparing copper alloy powder according to claim 4, characterized in that: In step S3, the material of the smelting crucible is a prefabricated corundum crucible coated with zirconium oxide; during the raw material smelting process, medium frequency induction heating is adopted to gradually increase the temperature for smelting. When the metal is completely melted, the heating power is reduced and a slag-forming agent is added to the smelting crucible.
7. A method for preparing copper alloy powder according to claim 4, characterized in that: In step S3, while the metal is being smelted, the tundish is heated and kept warm by gradually increasing the temperature.
8. A method for preparing copper alloy powder according to claim 4, characterized in that: The pouring temperature of step S5 is 1430-1470°C, and the pouring point of the copper alloy melt is located between the inner ring edge of the funnel-shaped ladle pouring port of the tundish and the 1 / 3 position of the inner ring edge extending outward.
9. A method for preparing copper alloy powder according to claim 4, characterized in that: In step S5, the atomization pressure is 4-5 MPa.
10. A method for preparing copper alloy powder according to claim 4, characterized in that: In step S6, the powder is classified by an integrated airflow classification device, the fan frequency is 40-50 Hz, the classification frequency is 8-10 Hz, and the particle size distribution requirements are: D10: 15-25 μm, D50: 30-40 μm, D90: 53-58 μm.
Citation Information
Cited By
Manufacturing method and device of spray-formed anticorrosive coating
CN120158698A
Method and apparatus for manufacturing an anti-corrosion coating by spray forming
CN120158698B