Nano-micro-scale mixed silver powder and preparation method and application thereof
By adding seed additives and alkaline carboxylate salts in two times and using metal chelating agents, the complexity and stability of photovoltaic composite silver powder preparation technology is solved, and the simplicity of nano- and micro-scale silver powder is achieved. The regulation of preparation and nano powder proportion is suitable for the field of conductive silver paste.
Patent Information
- Application Number
- CN202410963857.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The preparation technology of photovoltaic composite silver powder is complex, and it needs to consider a variety of factors. It is highly required for stability and durability in long-term use. It is difficult for the prior art to provide simple and stable preparation methods to achieve monodispersity and nano powder proportion. Regulation.
By configuring the silver nitrate reaction solution, reducing agent solution, dispersant solution and seed additive solution, the seed additive solution and alkaline carboxylate salt were added in two times, and the reaction was continued after adding the metal chelating agent to control the silver nitrate. The injection time and proportion of the reaction solution are used to improve dispersion and realize the mixing and adjustment of nano-scale and micro-scale silver powder.
It has achieved stable regulation with a simple process and a proportion of nano-powder between 10% and 50%, and obtained nano-scale and micro-scale mixed silver powder with good monodispersity, which is suitable for the preparation of conductive silver pastes.
Smart Images

Figure CN118905234A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of precious metal raw material powders, and in particular to a nano-micro mixed silver powder, a preparation method and application thereof. Background Art
[0002] Nano silver powder and micron silver powder are widely used materials. They have good conductivity, antibacterial properties and adjustable optical properties. They are widely used in electronics, medical, textile, food and other fields. With the continuous development of science and technology, the application of nano and micron silver powder in various fields has been continuously expanded and deepened.
[0003] In particular, nano and micron silver powders are widely used in the preparation of conductive materials in the electronics field. Since silver has high conductivity, nano silver powder and micron silver powder are usually mixed together to prepare a more efficient conductive paste for use in printed circuit boards, flexible displays and other fields. The largest demand for composite silver powder is in the photovoltaic field. Currently, with the upgrade and iteration of photovoltaic cells, the demand for composite silver powder is increasing.
[0004] However, the preparation technology of photovoltaic composite silver powder is relatively complex and has certain technical difficulties. The influence of various factors needs to be considered in the preparation process of photovoltaic composite silver powder. For example, the size, shape, and distribution of powder particles have an important influence on its performance and need to be carefully controlled during the synthesis process. In addition, the interaction between different materials needs to be considered to ensure that the composite effect between silver powder and other materials is maximized. In addition, the stability and durability of photovoltaic composite silver powder also need to be considered in the application field. As a long-term energy conversion device, solar cells have high requirements on the stability and durability of materials. Therefore, in the preparation process of photovoltaic composite silver powder, it is necessary to consider the problems such as photothermal performance, hygrothermal performance, mechanical properties, etc. that may be encountered during long-term use to ensure that it can maintain good performance in complex environments.
[0005] In summary, the preparation technology of photovoltaic composite silver powder is relatively difficult, and it is challenging to comprehensively consider multiple factors such as material synthesis, structural design, and performance regulation. At present, it is urgent to provide a preparation method with simple process and stable adjustment means, and at the same time, the prepared composite silver powder has good monodispersity and the proportion of nanopowder can be adjusted.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The purpose of the present invention is to provide a nano-micro mixed silver powder, a preparation method and application thereof, aiming to provide a simple process, and the proportion of nano powder can be stably regulated.
[0008] The present invention is achieved in that:
[0009] In a first aspect, the present invention provides a method for preparing nano-micro mixed silver powder, comprising:
[0010] A silver nitrate reaction solution, a reducing agent solution, a dispersant solution and a seeding agent solution are prepared, wherein the preparation process of the seeding agent solution comprises: mixing the silver nitrate aqueous solution, the reducing agent and the dispersant for reaction;
[0011] Injecting the silver nitrate reaction solution and the reducing agent solution into the dispersant solution, and when the injection amount of the silver nitrate reaction solution reaches 30%-50% of the total volume of the silver nitrate reaction solution, adding 40%-60% of the seed crystal auxiliary solution for reaction;
[0012] When the injection amount of the silver nitrate reaction solution reaches 50%-70% of the total volume of the silver nitrate reaction solution, the remaining seeding auxiliary solution and the alkaline carboxylate are added;
[0013] After the injection of the silver nitrate reaction solution is completed, a metal chelating agent is added to continue the reaction.
[0014] In an optional embodiment, the total injection time of the silver nitrate reaction solution and the reducing agent solution is controlled to be 8 min-12 min, and the reaction is continued for 2 min-5 min after the metal chelating agent is added.
[0015] In an optional embodiment, after adding the metal chelating agent and continuing the reaction for 2 min-5 min, stirring for 25 min-35 min, then performing solid-liquid separation to obtain wet powder, and then washing and drying the wet powder;
[0016] Preferably, a surfactant is added before solid-liquid separation or to the obtained wet powder;
[0017] More preferably, the surfactant is selected from at least one of oleic acid, sodium oleate and potassium oleate.
[0018] In an optional embodiment, the preparation process of the seeding agent solution includes: mixing a silver nitrate aqueous solution with a concentration of 0.05 mmol / L-0.15 mmol / L with a reducing agent and a dispersing agent, and reacting at 50° C.-150° C. for 20 min-40 min; controlling the mass ratio of the silver nitrate aqueous solution, the reducing agent and the dispersing agent to be 10:(0.2-0.3):(0.5-1.5);
[0019] Preferably, when preparing the seeding agent solution, the reducing agent used is at least one selected from ethanolamine, diethanolamine and triethanolamine;
[0020] Preferably, when preparing the seed adjuvant solution, the dispersant used is at least one selected from polyvinyl pyrrolidone, gum arabic, gelatin and Tween.
[0021] In an optional embodiment, the concentration of the silver nitrate reaction solution is 1 mol / L-2 mol / L, the mass fraction of the reducing agent solution is 18-22%, and the injection rates of the silver nitrate reaction solution and the reducing agent solution are both 8 mL / min-12 mL / min;
[0022] Preferably, the reducing agent solution is obtained by mixing a reducing agent and water, and the reducing agent is selected from at least one of ascorbic acid, glucose and sodium hypophosphite.
[0023] In an optional embodiment, the dispersant solution is obtained by mixing a dispersant and water, and the dispersant is selected from at least one of polyvinyl pyrrolidone, gelatin, gum arabic and Tween;
[0024] Preferably, the dispersant used to prepare the dispersant solution comprises polyvinyl pyrrolidone, gelatin, gum arabic and Tween, and the mass ratio of polyvinyl pyrrolidone, gelatin, gum arabic and Tween is 8:(0.5-1.5):(0.5-1.5):(0.5-1.5);
[0025] Preferably, the mass proportion of the total amount of dispersant in the dispersant solution is 2%-5%, and the volume ratio of the dispersant solution to the silver nitrate reaction solution is (0.5-3):1.
[0026] In an optional embodiment, the alkaline carboxylate is selected from at least one of sodium stearate, sodium citrate and sodium acetate;
[0027] Preferably, the alkaline carboxylate is added in the form of an aqueous solution, the mass fraction of the alkaline carboxylate aqueous solution is controlled to be 8%-12%, and the volume ratio of the added alkaline carboxylate aqueous solution to the silver nitrate reaction solution is 100:(0.5-2).
[0028] In an optional embodiment, the metal chelator is selected from at least one of ethylenediaminetetraacetic acid, ethylene glycol tetraacetic acid and tetramethylethylenediamine;
[0029] Preferably, the metal chelating agent is added in the form of an aqueous solution, the mass fraction of the metal chelating agent aqueous solution is controlled to be 8%-12%, and the volume ratio of the added metal chelating agent aqueous solution to the silver nitrate reaction solution is 100:(0.5-2).
[0030] In a second aspect, the present invention provides a nano-micro mixed silver powder prepared by any one of the preparation methods described in the aforementioned embodiments.
[0031] In a third aspect, the present invention provides the use of the nano-micro mixed silver powder of the aforementioned embodiment in the preparation of a conductive silver paste.
[0032] The present invention has the following beneficial effects: by adding the seed crystal auxiliary solution twice, when the injection amount of the silver nitrate reaction solution reaches 30%-50% of the total volume of the silver nitrate reaction solution, 40%-60% of the seed crystal auxiliary solution is added for reaction; when the injection amount of the silver nitrate reaction solution reaches 50%-70% of the total volume of the silver nitrate reaction solution, the remaining seed crystal auxiliary solution and alkaline carboxylate are added; after the injection of the silver nitrate reaction solution is completed, a metal chelating agent is added to continue the reaction. The crystal auxiliary agent and the metal chelating agent are respectively a particle size control agent and a nano powder ratio adjuster, and an alkaline carboxylate regulator is introduced at the same time, and a composite silver powder can be obtained by reacting with the mother liquor solution at an appropriate time. The preparation method provided by the present invention is simple and easy to operate, and the ratio of nano silver powder to micron-level silver powder is changed, and the final nano silver powder ratio is adjustable between 10%-50%, and the dispersibility is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0034] Figure 1 This is an electron microscope image of the nano- and micro-mixed silver powder prepared in Example 1;
[0035] Figure 2 This is an electron microscope image of the nano- and micro-mixed silver powder prepared in Example 2;
[0036] Figure 3 This is an electron microscope image of the nano- and micro-mixed silver powder prepared in Example 3;
[0037] Figure 4 This is an electron microscope image of the nano- and micro-mixed silver powder prepared in Comparative Example 1;
[0038] Figure 5 This is an electron microscope image of the nano- and micro-mixed silver powder prepared in Comparative Example 2;
[0039] Figure 6 This is an electron microscope image of the nano-micron mixed silver powder prepared in Comparative Example 3. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0041] The embodiment of the present invention provides a method for preparing nano-micro mixed silver powder, comprising the following steps:
[0042] S1. Prepare seed crystal auxiliary solution
[0043] The preparation process of the seed crystal auxiliary agent solution comprises: mixing and reacting a silver nitrate aqueous solution, a reducing agent and a dispersant to obtain a seed crystal auxiliary agent solution containing nano silver.
[0044] In some embodiments, the preparation process of the seeding agent solution includes: mixing a silver nitrate aqueous solution with a concentration of 0.05 mmol / L-0.15 mmol / L with a reducing agent and a dispersing agent, reacting at 50°C-150°C for 20min-40min; controlling the mass ratio of the silver nitrate aqueous solution, the reducing agent and the dispersing agent to be 10:(0.2-0.3):(0.5-1.5). By adjusting the concentration of the silver nitrate aqueous solution, as well as the reaction conditions such as the dosage ratio of the silver nitrate aqueous solution, the reducing agent and the dispersing agent, the silver particles in the generated seeding agent solution are nanometer-sized, which is convenient for continued growth as seeds in subsequent reactions.
[0045] Specifically, the concentration of the silver nitrate aqueous solution can be 0.05mmol / L, 0.08mmol / L, 0.10mmol / L, 0.12mmol / L, 0.15mmol / L, etc., and the mass ratio of the silver nitrate aqueous solution, the reducing agent and the dispersant can be 10:0.20:0.5, 10:0.23:0.8, 10:0.25:1.0, 10:0.28:1.2, 10:0.30:1.5, etc. The reaction temperature can be 50°C, 80°C, 100°C, 120°C, 150°C, etc.; the reaction time can be 20min, 25min, 30min, 35min, 40min, etc.
[0046] In some embodiments, when preparing the seed adjuvant solution, the reducing agent used is selected from at least one of ethanolamine, diethanolamine and triethanolamine, and the reducing agent can be any one or more of the above; the dispersant used is selected from at least one of polyvinyl pyrrolidone (PVP), gum arabic, gelatin and Tween, and the dispersant can be any one or more of the above, such as PVP K30.
[0047] S2. Prepare silver nitrate reaction solution, reducing agent solution and dispersant solution
[0048] The silver nitrate reaction solution is obtained by mixing silver nitrate and water. The concentration of the silver nitrate reaction solution is controlled to be 1 mol / L-2 mol / L, such as 1.0 mol / L, 1.3 mol / L, 1.5 mol / L, 1.8 mol / L, 2.0 mol / L, etc.
[0049] The reducing agent solution is obtained by mixing a reducing agent and water, wherein the reducing agent is selected from at least one of ascorbic acid, glucose and sodium hypophosphite, and may be any one or more of the above. The mass fraction of the reducing agent solution is 18-22%, such as 18%, 19%, 20%, 21%, 22%, etc.
[0050] The dispersant solution is obtained by mixing a dispersant and water, wherein the dispersant is selected from at least one of polyvinyl pyrrolidone, gelatin, gum arabic and Tween, and the dispersant may be any one or more of the above. The mass proportion of the total amount of the dispersant in the dispersant solution is 2%-5%, such as 2%, 3%, 4%, 5%, etc.
[0051] In some embodiments, the dispersant used to prepare the dispersant solution includes polyvinyl pyrrolidone, gelatin, gum arabic and Tween, and the mass ratio of polyvinyl pyrrolidone, gelatin, gum arabic and Tween is 8: (0.5-1.5): (0.5-1.5): (0.5-1.5), such as 8: 0.5: 0.5: 0.5, 8: 1.0: 1.0: 1.0, 8: 1.5: 1.5: 1.5, etc. By adjusting the type and amount of the dispersant, the prepared composite silver powder has better dispersibility.
[0052] Furthermore, the volume ratio of the dispersant solution to the silver nitrate reaction solution is (0.5-3):1, such as 0.5:1, 1.0:1, 1.5:1, 2.0:1, 2.5:1, 3.0:1, etc. The reducing agent solution and the silver nitrate reaction solution should be injected into the reactor simultaneously during the reaction process, and the volumes of the two can be approximately the same, and they are controlled to be injected into the reactor at approximately the same flow rate.
[0053] S3, step-by-step reaction
[0054] The silver nitrate reaction solution and the reducing agent solution are injected into the dispersant solution, and when the injection amount of the silver nitrate reaction solution reaches 30%-50% of the total volume of the silver nitrate reaction solution, 40%-60% of the seed crystal auxiliary solution is added for reaction; when the injection amount of the silver nitrate reaction solution reaches 50%-70% of the total volume of the silver nitrate reaction solution, the remaining seed crystal auxiliary solution and alkaline carboxylate are added; after the injection of the silver nitrate reaction solution is completed, a metal chelating agent is added to continue the reaction. By controlling the timing of adding the seed crystal auxiliary solution twice, coordinating the addition of the alkaline carboxylate and the metal chelating agent, the crystal auxiliary agent and the metal chelating agent are respectively used as the particle size control agent and the nano powder proportion adjustment agent, and at the same time, the alkaline carboxylate regulator is introduced, and the composite silver powder can be obtained by reacting with the mother liquor solution at an appropriate time.
[0055] Specifically, when the injection amount of the silver nitrate reaction solution reaches 30%-50% (such as 30%, 40%, 50%, etc.) of the total volume of the silver nitrate reaction solution, 40%-60% (such as 40%, 50%, 60%, etc. by mass) of the seeding agent solution is added. When the injection amount of the silver nitrate reaction solution reaches 50%-70% (such as 50%, 60%, 70%, etc.) of the total volume of the silver nitrate reaction solution, the remaining seeding agent solution and alkaline carboxylate are added. If the desired product is mainly nanoparticles, the timing of the second addition of the seeding agent solution can be advanced (such as the injection amount of the silver nitrate reaction solution reaches 80%); if the desired product is mainly nanoparticles, the timing of the second addition of the seeding agent solution can be delayed (such as the injection amount of the silver nitrate reaction solution reaches 90%).
[0056] In some embodiments, the total injection time of the silver nitrate reaction solution and the reducing agent solution is controlled to be 8 min-12 min, such as 8 min, 9 min, 10 min, 11 min, 12 min, etc.; the reaction time after adding the metal chelating agent is 2 min-5 min, such as 2 min, 3 min, 4 min, 5 min, etc. The injection rate of the silver nitrate reaction solution and the reducing agent solution is 8 mL / min-12 mL / min, such as 8 mL / min, 9 mL / min, 10 mL / min, 11 mL / min, 12 mL / min, etc. The particle size distribution of the final product can be controlled by accurately controlling the total addition time and reaction time of the silver nitrate reaction solution.
[0057] In some embodiments, the alkaline carboxylate is selected from at least one of sodium stearate, sodium citrate and sodium acetate, and the alkaline carboxylate can be any one or more of the above. The alkaline carboxylate is added in the form of an aqueous solution, and the mass fraction of the alkaline carboxylate aqueous solution is controlled to be 8%-12%, and the volume ratio of the added alkaline carboxylate aqueous solution to the silver nitrate reaction solution is 100: (0.5-2). The addition of alkaline carboxylates can slow down particle growth and control the particle size of the product, and its dosage is preferably within the above range. Specifically, the mass fraction of the alkaline carboxylate aqueous solution can be 8%, 9%, 10%, 11%, 12%, etc., and the volume ratio of the added alkaline carboxylate aqueous solution to the silver nitrate reaction solution can be 100: 0.5, 100: 1.0, 100: 1.5, 100: 2.0, etc., and the pH value of the silver powder mother liquor after the addition of the alkaline carboxylate is controlled to be approximately 1-3.
[0058] In some embodiments, the metal chelator is selected from at least one of ethylenediaminetetraacetic acid, ethylene glycol tetraacetic acid and tetramethylethylenediamine, and can be any one or more of the above. The metal chelator is added in the form of an aqueous solution, and the mass fraction of the metal chelator aqueous solution is controlled to be 8%-12%, and the volume ratio of the added metal chelator aqueous solution to the silver nitrate reaction solution is 100: (0.5-2). The addition of the metal chelator can play a role in passivating the surface of the silver powder, reducing the activity of the silver powder, and preventing the silver powder from sticking. Specifically, the mass fraction of the metal chelator aqueous solution is 8%, 9%, 10%, 11%, 12%, etc., and the volume ratio of the added metal chelator aqueous solution to the silver nitrate reaction solution can be 100: 0.5, 100: 1.0, 100: 1.5, 100: 2.0, etc.
[0059] S4. Post-processing
[0060] After adding the metal chelating agent and continuing the reaction for 2-5 minutes, stir for 25-35 minutes to stabilize the system, then perform solid-liquid separation to obtain wet powder, and wash and dry the wet powder. The residual dispersant on the surface is removed by washing, and a nano-scale and micron-scale mixed silver powder is obtained after drying. Specifically, the stirring time can be 25 minutes, 30 minutes, 35 minutes, etc.; the solid-liquid separation method is not limited, and it can be a centrifugal separation method; the washing method is not limited and can be multiple water washings.
[0061] In some embodiments, a surfactant is added before solid-liquid separation or to the obtained wet powder to prevent the silver powder from sticking during the drying process. The surfactant can be added before stirring for 25 min to 35 min or can be added to the obtained wet powder.
[0062] In some embodiments, the surfactant is selected from at least one of oleic acid, sodium oleate and potassium oleate, and the surfactant can be any one or more of the above.
[0063] The embodiment of the present invention provides a nano-micro mixed silver powder, which is prepared by the above-mentioned preparation method, and the process is simple and easy, and the proportion of nano silver powder in the obtained mixed silver powder can be stably adjusted. The nano-micro mixed silver powder can be used in the field of preparing conductive silver paste, and the proportion of nano silver powder in the product can be controlled according to the specific application scenario.
[0064] The preparation method provided by the embodiment of the present invention can synthesize nano- and micron-mixed silver powder in one step. The average particle size of the nano silver powder is between 200-400 nanometers, and the average particle size of the micron silver powder is between 1.0-1.5 microns. The monodispersity is good and the proportion of the nano powder is adjustable. The invention has broad application prospects in the field of conductive silver paste.
[0065] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0066] Example 1
[0067] This embodiment provides a method for preparing nano-micro mixed silver powder, and the specific steps are as follows:
[0068] (1) At room temperature (25°C), take 20 g of 0.1 mmol / L silver nitrate solution, add 0.5 g of ethanolamine, and then add 2 g of PVP K30 powder, and ripen in a constant temperature oil bath at 100.0°C for 30 min to obtain a brown seed auxiliary agent solution containing nanosilver.
[0069] (2) Weigh 25 g of silver nitrate and 92 g of deionized water, stir until completely dissolved, and obtain a silver nitrate solution with a volume of about 100 mL and a concentration of about 1.5 mol / L; weigh 20 g of ascorbic acid and 80 g of deionized water, stir until completely dissolved, and obtain a reducing agent solution with a volume of 100 mL and a mass fraction of 20%; weigh 4 g of polyvinyl pyrrolidone K30 (i.e., PVP K30), 0.5 g of gelatin, 0.5 g of gum arabic, 0.5 g of Tween, and 150 g of deionized water, stir until completely dissolved, and obtain a dispersant solution.
[0070] (3) Under stirring at 400 rpm, the silver nitrate solution and reducing agent solution obtained in step (2) are injected at a flow rate of 10 mL / min, and 11.1 g of seeding agent solution is added before the silver nitrate solution is injected. When the injected volume of the silver nitrate solution reaches 30.0% of the total volume, the remaining seeding agent solution is added, and 1 mL of 10% mass fraction of sodium stearate is added at the same time. After the injection of the silver nitrate solution is completed, 1 mL of 10% mass fraction of ethylenediaminetetraacetic acid (EDTA) solution is immediately added, and stirring is continued for 30 minutes.
[0071] (4) Finally, the mother liquor is centrifuged at 4000 rpm to obtain wet powder, which is then washed with deionized water to remove the surface dispersant and dried to obtain a nano- and micro-scale mixed silver powder.
[0072] The nano-scale and micro-scale mixed silver powder prepared in this embodiment is as follows Figure 1 As shown, it can be seen that the silver powder prepared in this embodiment is relatively nano-sized, because the remaining seeds and the metal complexing agent solution EDTA are added after 30% of the silver nitrate is injected, so that the redox reaction is slowed down, and more nanoparticles and fewer micron particles are generated.
[0073] Example 2
[0074] This embodiment provides a method for preparing nano-micro mixed silver powder, and the specific steps are as follows:
[0075] (1) At room temperature (25°C), take 20 g of 0.1 mmol / L silver nitrate solution, add 0.5 g of ethanolamine, and then add 2 g of PVP K30 powder, and ripen in a constant temperature oil bath at 150°C for 30 min to obtain a brown seed solution containing nanosilver.
[0076] (2) Weigh 25 g of silver nitrate and 92 g of deionized water, stir until completely dissolved, and obtain a silver nitrate solution with a volume of about 100 mL and a concentration of about 1.5 mol / L; weigh 20 g of ascorbic acid and 80 g of deionized water, stir until completely dissolved, and obtain a reducing agent solution with a volume of 100 mL and a mass fraction of 20%; weigh 4 g of polyvinyl pyrrolidone K30, 0.5 g of gelatin, 0.5 g of gum arabic, 0.5 g of Tween, and 150 g of deionized water, stir until completely dissolved, and obtain a dispersant solution.
[0077] (3) Under stirring at 400 rpm, the silver nitrate solution and reducing agent solution obtained in step (2) are injected at a flow rate of 10 mL / min, and 11.1 g of seeding agent solution is added before the silver nitrate solution is injected. When the injection volume of the silver nitrate solution reaches 40.0% of the total volume, the remaining seeding agent solution is added, and 1 mL of 10% mass fraction of sodium stearate is added at the same time. After the injection of the silver nitrate solution is completed, 1 mL of 10% mass fraction of ethylenediaminetetraacetic acid (EDTA) solution is immediately added, and stirring is continued for 30 minutes.
[0078] (4) The mother liquor is centrifuged at 4000 rpm to obtain wet powder, which is then washed with deionized water to remove the surface dispersant and dried to obtain a mixed nano- and micro-scale silver powder.
[0079] The nano-scale and micro-scale mixed silver powder prepared in this embodiment is as follows Figure 2 As shown, it can be seen that the nano-scale silver powder prepared in this embodiment accounts for less than that in Example 1, because the surfactant and the metal complexing agent are added later, and the early silver powder particles are enlarged into micron-scale particles.
[0080] Example 3
[0081] This embodiment provides a method for preparing nano-micro mixed silver powder, and the specific steps are as follows:
[0082] (1) At room temperature (25°C), take 20 g of 0.1 mmol / L silver nitrate solution, add 0.5 g of ethanolamine, and then add 2 g of PVP K30 powder, and ripen in a constant temperature oil bath at 150°C for 30 min to obtain a brown seed solution containing nanosilver.
[0083] (2) Weigh 25 g of silver nitrate and 92 g of deionized water, stir until completely dissolved, and obtain a silver nitrate solution with a volume of about 100 mL and a concentration of about 1.5 mol / L; weigh 20 g of ascorbic acid and 80 g of deionized water, stir until completely dissolved, and obtain a reducing agent solution with a volume of 100 mL and a mass fraction of 20%; weigh 4 g of polyvinyl pyrrolidone K30, 0.5 g of gelatin, 0.5 g of gum arabic, 0.5 g of Tween, and 150 g of deionized water, stir until completely dissolved, and obtain a dispersant solution.
[0084] (3) Under stirring at 400 rpm, the silver nitrate solution and reducing agent solution obtained in step (2) are injected at a flow rate of 10 mL / min, and 11.1 g of seeding agent solution is added before the silver nitrate solution is injected. When the injection volume of the silver nitrate solution reaches 50.0% of the total volume, the remaining seeding agent solution is added, and 1 mL of 10% mass fraction of sodium stearate is added at the same time. After the injection of the silver nitrate solution is completed, 1 mL of 10% mass fraction of ethylenediaminetetraacetic acid (EDTA) solution is immediately added, and stirring is continued for 30 minutes.
[0085] (4) The mother liquor is centrifuged at 4000 rpm to obtain wet powder, which is then washed with deionized water to remove the surface dispersant and dried to obtain a mixed nano- and micro-scale silver powder.
[0086] The nano-scale and micro-scale mixed silver powder prepared in this embodiment is as follows Figure 3 As shown, it can be seen that the silver powder prepared in this embodiment is mostly micron-sized, and the principle is the same as that of Example 2.
[0087] Example 4
[0088] The only difference from Example 1 is that the sodium stearate in step (3) is replaced by an equal amount of sodium citrate (i.e., equal concentration and equal volume).
[0089] Example 5
[0090] The only difference from Example 1 is that the sodium stearate in step (3) is replaced by an equal amount of sodium acetate; and the complexing agent ethylenediaminetetraacetic acid (EDTA) is replaced by an equal amount of tetramethylethylenediamine.
[0091] Example 6
[0092] The only difference from Example 1 is that the sodium stearate in step (3) is replaced by half an equal amount of sodium acetate and half an equal amount of sodium citrate; and the complexing agent ethylenediaminetetraacetic acid (EDTA) is replaced by an equal amount of ethylene glycol tetraacetic acid.
[0093] Example 7
[0094] The only difference from Example 1 is that the silver nitrate solution and the reducing agent solution are injected at a flow rate of 20 mL / min, and the total injection time is halved.
[0095] Comparative Example 1
[0096] The only difference from Example 1 is that no ethylenediaminetetraacetic acid (EDTA) solution was added during the preparation process.
[0097] The nano-scale and micro-scale mixed silver powder prepared in this comparative example is Figure 4 As shown, it can be seen that the silver powder is mainly in the micron level. Because there is no participation of metal chelating agent, the overall oxidation rate is slow, the silver powder particles are easy to become larger and due to the secondary addition of seed crystals, there will be large and small particles.
[0098] Comparative Example 2
[0099] The only difference from Example 1 is that the remaining seed auxiliary agent solution is not added in step (3).
[0100] The nano-scale and micro-scale mixed silver powder prepared in this comparative example is Figure 5 As shown, it can be seen that the silver powder is mainly in the micron level, and due to the small number of seed crystals, the overall particle size becomes larger.
[0101] Comparative Example 3
[0102] The only difference from Example 1 is that in step (3), the seeding auxiliary agent solution is added at one time.
[0103] The nano-scale and micro-scale mixed silver powder prepared in this comparative example is Figure 6 As shown, it can be seen that the silver powder is mainly in the micron size, and due to the single addition of the seed crystal, the powder has different sizes.
[0104] Test Example 1
[0105] The performance of the nano-scale and micro-scale mixed silver powder prepared in the test examples and comparative examples is shown in Table 1.
[0106] Test method for printing performance of slurry: 9.21g of powder, 0.71g of ethyl cellulose resin, 0.05g of silicone oil and 0.03g of dispersant are synthesized into slurry in a fixed proportion, and the slurry is ground by a three-roll mill and then tested for fineness and viscosity.
[0107] Table 1 Performance of nano-scale and micro-scale mixed silver powder prepared in Examples and Comparative Examples
[0108] Group 0.5RPM(mPa.s) 1.0RPM(mPa.s) 5.0RPM(mPa.s) Fineness(um) Example 1 369792.16 277822.24 134452.94 5.0 Example 2 298928.64 239077.76 125253.95 7.0 Example 3 247663.12 180283.52 96977.47 7.5 Example 4 312791.68 259022.24 145940.57 6.0 Example 5 336954.24 226540.48 107538.88 7.5 Example 6 268928.63 193521.28 98902.49 7.0 Example 7 387394.88 269678.40 116253.95 7.5 Comparative Example 1 427455.36 289922.40 109823.80 10 Comparative Example 2 268703.36 204315.20 141762.78 15 Comparative Example 3 580706.56 447886.88 168752.00 12.5
[0109] Through the examples, it can be seen that as the proportion of coarse powder in the powder increases, the viscosity decreases at the same speed under the same formula, and the fineness increases slightly, but both are less than 10. This shows that the powder prepared by this scheme can effectively adjust the viscosity of the slurry and meet the mesh number of the sieve. In the various comparative examples, due to the small proportion of nano-scale particles in the powder, the fineness is obviously larger (greater than 10), and the overall viscosity of the slurry is also larger.
[0110] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing nano-micro mixed silver powder, characterized in that: include: A silver nitrate reaction solution, a reducing agent solution, a dispersant solution and a seeding agent solution are prepared, wherein the preparation process of the seeding agent solution comprises: mixing the silver nitrate aqueous solution, the reducing agent and the dispersant for reaction; Injecting the silver nitrate reaction solution and the reducing agent solution into the dispersant solution, and when the injection amount of the silver nitrate reaction solution reaches 30%-50% of the total volume of the silver nitrate reaction solution, adding 40%-60% of the seed crystal auxiliary solution for reaction; When the injection amount of the silver nitrate reaction solution reaches 50%-70% of the total volume of the silver nitrate reaction solution, the remaining seeding auxiliary solution and alkaline carboxylate are added; After the injection of the silver nitrate reaction solution is completed, a metal chelating agent is added to continue the reaction.
2. The preparation method according to claim 1, characterized in that: The total injection time of the silver nitrate reaction solution and the reducing agent solution is controlled to be 8 min-12 min, and the reaction is continued for 2 min-5 min after the metal chelating agent is added.
3. The preparation method according to claim 2, characterized in that: After adding the metal chelating agent and continuing the reaction for 2-5 minutes, stirring for 25-35 minutes, and then performing solid-liquid separation to obtain wet powder, and then washing and drying the wet powder; Preferably, a surfactant is added before solid-liquid separation or to the obtained wet powder; More preferably, the surfactant is selected from at least one of oleic acid, sodium oleate and potassium oleate.
4. The preparation method according to claim 1, characterized in that: The preparation process of the seeding auxiliary agent solution includes: mixing a silver nitrate aqueous solution with a concentration of 0.05mmol / L-0.15mmol / L with the reducing agent and the dispersing agent, and reacting at 50°C-150°C for 20min-40min; controlling the mass ratio of the silver nitrate aqueous solution, the reducing agent and the dispersing agent to be 10:(0.2-0.3):(0.5-1.5); Preferably, when preparing the seeding auxiliary agent solution, the reducing agent used is at least one selected from ethanolamine, diethanolamine and triethanolamine; Preferably, when preparing the seed adjuvant solution, the dispersant used is at least one selected from polyvinyl pyrrolidone, gum arabic, gelatin and Tween.
5. The preparation method according to claim 1, characterized in that: The concentration of the silver nitrate reaction solution is 1 mol / L-2 mol / L, the mass fraction of the reducing agent solution is 18-22%, and the injection rates of the silver nitrate reaction solution and the reducing agent solution are both 8 mL / min-12 mL / min; Preferably, the reducing agent solution is obtained by mixing a reducing agent and water, and the reducing agent is selected from at least one of ascorbic acid, glucose and sodium hypophosphite.
6. The preparation method according to claim 1 or 5, characterized in that: The dispersant solution is obtained by mixing a dispersant and water, wherein the dispersant is selected from at least one of polyvinyl pyrrolidone, gelatin, gum arabic and Tween; Preferably, the dispersant used to prepare the dispersant solution comprises polyvinyl pyrrolidone, gelatin, gum arabic and Tween, and the mass ratio of polyvinyl pyrrolidone, gelatin, gum arabic and Tween is 8: (0.5-1.5): (0.5-1.5): (0.5-1.5); Preferably, the mass ratio of the total amount of dispersant in the dispersant solution is 2%-5%, and the volume ratio of the dispersant solution to the silver nitrate reaction solution is (0.5-3):
1.
7. The preparation method according to claim 1, characterized in that: The alkaline carboxylate is selected from at least one of sodium stearate, sodium citrate and sodium acetate; Preferably, the alkaline carboxylate is added in the form of an aqueous solution, the mass fraction of the alkaline carboxylate aqueous solution is controlled to be 8%-12%, and the volume ratio of the added alkaline carboxylate aqueous solution to the silver nitrate reaction solution is 100:(0.5-2).
8. The preparation method according to claim 1, characterized in that: The metal chelating agent is selected from at least one of ethylenediaminetetraacetic acid, ethylene glycol tetraacetic acid and tetramethylethylenediamine; Preferably, the metal chelating agent is added in the form of an aqueous solution, the mass fraction of the metal chelating agent aqueous solution is controlled to be 8%-12%, and the volume ratio of the metal chelating agent aqueous solution to the silver nitrate reaction solution is 100:(0.5-2).
9. A nano-micro mixed silver powder, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 8.
10. Use of the nano-micro mixed silver powder according to claim 9 in preparing conductive silver paste.
Citation Information
Cited By
Method for preparing nano flake silver powder, flake silver powder and application
CN119772162A