Lignin activated carbon capacitive deionization anode electrode material as well as preparation method and application thereof

By combining lignin with Bi/BiOCl or Ag/AgCl system, an efficient lignin activated carbon capacitor deionized anode material is prepared, which solves the problems of high cost, low adsorption capacity and poor stability in the prior art, and achieves low Cost, high adsorption capacity and long life capacitive deionization effect.

CN118993260AActive Publication Date: 2024-11-22HUANGGANG NORMAL UNIV

Patent Information

Application Number
CN202411267513.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-22
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

In the existing capacitor deionization technology, the anode material has high production cost, low adsorption capacity, poor stability, and strong dependence on fossil raw materials, making it difficult to meet the needs of efficient energy-saving and desalination technology.

Method used

Using lignin activated carbon as capacitive deionized anode material, Bi@lignin, Ag@lignin, BiOCl@lignin composite materials are prepared by combining with Bi/BiOCl or Ag/AgCl system, and by solvent exchange and hydrothermal reaction, and Carbonization under an inert atmosphere forms an efficient and stable anode material.

Benefits of technology

It realizes the deionized anode material of lignin activated carbon capacitor with low raw material cost, high adsorption capacity and long service life, reducing production difficulty and cost, improving the mechanical strength and physical and chemical stability of the material, and is suitable for capacitor deionized desalination technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993260A_ABST
    Figure CN118993260A_ABST
Patent Text Reader

Abstract

The invention discloses a lignin activated carbon capacitive deionization anode electrode material and a preparation method and application thereof, and belongs to the technical field of capacitive deionization. The method comprises the following steps: (1) preparing a corresponding composite material according to the components of the lignin activated carbon capacitive deionization anode electrode material; (2) carbonizing the composite material; and (3) obtaining the lignin activated carbon capacitive deionization anode electrode material. The method has the advantages of being convenient in process, low in raw material cost, wide in raw material source and environment-friendly. The prepared lignin activated carbon capacitive deionization anode electrode material has the characteristics of good stability, long service life and high adsorption capacity, and has a good prospect in the field of capacitive deionization desalination.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of capacitor deionization, and in particular to a lignin activated carbon capacitor deionization anode electrode material and a preparation method and application thereof. Background Art

[0002] With the rapid growth of population and rapid economic development, the problem of water shortage has become increasingly prominent and has become one of the core issues to be solved. High-efficiency and energy-saving desalination technology is an effective measure to solve the problem of fresh water shortage. Capacitive deionization technology has become one of the most promising desalination technologies due to its advantages such as low energy consumption, simple equipment, and green environmental protection. However, the current production cost of capacitive deionization electrodes is high, the types of anode materials are relatively small, and the adsorption capacity is relatively low, which restricts the development of this type of desalination technology.

[0003] On the one hand, for materials that store chloride ions through conversion reactions, such as Ag / AgCl, Bi / BiOCl, etc., due to their large adsorption capacity, they are conducive to improving the adsorption performance of chloride ions by the anode, thereby improving the overall desalination capacity of hybrid capacitive deionization. However, the conversion reaction will cause a large volume expansion, causing its capacity to decay after multiple cycles, which is not conducive to its actual production application and is one of the problems that need to be solved in the current capacitive deionization technology.

[0004] For example, the Chinese invention patent with publication number CN112062229A discloses a Bi / MOF-derived porous carbon sphere composite material and its preparation method and application. The Bi / MOF-derived porous carbon sphere composite material is prepared by loading nano-scale metal Bi particles on the surface of N-doped MOF-derived porous carbon spheres. The Bi / MOF-derived porous carbon sphere composite material of the invention can effectively alleviate the volume expansion problem of Bi in the redox process by anchoring nano-scale metal Bi particles on MOF-derived carbon, enhance the stability of the electrode material, and reduce the electrode pulverization phenomenon. In the preparation of this step, N-doped MOF-derived porous carbide needs to be prepared, and bismuth oxide is reduced by a reducing agent to form a Bi / MOF-derived porous carbon sphere composite material, and the process is more complicated. In order to form a spherical morphology, zinc salts or iron salts are used in its preparation. Due to the crystallization kinetics of metal elements, the obtained pore structure is often disordered and irregular. Therefore, the requirements for precise control of pore size, density and distribution in the synthesis process of the MOF material are high, which also increases the difficulty and cost of production.

[0005] On the other hand, the raw materials of electrode materials at this stage are mostly from fossil raw materials, which are expensive and have complicated preparation processes. Therefore, it has become a trend to use renewable biomass materials to replace fossil energy materials. As a renewable biomass material, lignin is second only to cellulose in content and has the advantages of wide sources and low costs. Therefore, seeking suitable processes to use it in the field of capacitive deionization is of progressive significance in terms of reducing costs and reducing resource waste.

[0006] For example, the Chinese invention patent with publication number CN115463625A provides a silver nanowire-lignin-derived carbon composite aerogel and its preparation method and application. The silver nanowires are wrapped in lignin by rapid freezing to avoid the agglomeration of the silver nanowires. The unique adhesion, dispersibility and chelation of lignin evenly disperse the silver nanowires and form an interconnected network structure. The solvent is removed by freeze-drying to form a loose and porous mesoporous structure, which provides more active sites for ion adsorption and has good application prospects in the field of capacitive deionization. However, the silver nanowires required by this scheme have strict quality control requirements on the production process (such as polyol method, electrochemical method, vapor deposition method, template method, etc.) in the industry. It is currently difficult to obtain them in a general and simple way, and the preparation cost is still at a high level. In addition, the bonding strength between the functional material and the matrix in the encapsulated form is insufficient, and the electrode materials including aerogels and flexible membranes composed of two-dimensional nanomaterials also have technical problems such as insufficient mechanical strength, physical and chemical stability to be optimized, and short service life. They are poorly applicable in capacitive deionization devices based on electrochemical capture of ions, such as capacitive deionization, membrane capacitive deionization, and dual-ion electrochemical deionization, which further limits their application in the field of capacitive deionization.

[0007] In summary, a lignin activated carbon capacitor deionization anode electrode material and a preparation method with low raw material cost, environmental friendliness, good stability, long service life and high adsorption capacity are provided to solve the above-mentioned technical problems, which has positive significance for promoting the development of desalination technology. Summary of the invention

[0008] In view of the above-mentioned defects of the prior art, in the first aspect of the present invention, a method for preparing a lignin activated carbon capacitor deionization anode electrode material with convenient process, low raw material cost, wide source and environmental friendliness is provided, comprising the following steps: (1) Preparation of corresponding composite materials based on the components of lignin activated carbon capacitor deionization anode electrode materials: a. Mixing lignin, Bi precursor or Ag precursor with a solvent, dialyzing the resulting mixed solution in water to complete solvent exchange, and recovering the corresponding Bi@lignin composite material or Ag@lignin composite material; b. Mixing lignin, Ag precursor and solvent, dialyzing the resulting mixture in an aqueous solution of chloride salt to complete solvent exchange, and recovering the AgCl@lignin composite material; c. Mixing lignin, Bi precursor, chloride salt and solvent, and then performing a hydrothermal reaction; after the hydrothermal reaction is completed, recovering to obtain the BiOCl@lignin composite material; The Bi precursor, the Ag precursor, and the chloride salt are salts that are dissolved in a solvent and ionized; (2) Carbonization of composite materials: The Bi@lignin composite material, the Ag@lignin composite material, the AgCl@lignin composite material, and the BiOCl@lignin composite material are respectively subjected to calcination treatment in an inert atmosphere to complete carbonization, and Bi@lignin activated carbon anode material, BiOCl@lignin activated carbon anode material, Ag@lignin activated carbon anode material, and AgCl@lignin activated carbon anode material are obtained accordingly; (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material includes at least one of Bi@lignin activated carbon anode material, BiOCl@lignin activated carbon anode material, Ag@lignin activated carbon anode material, and AgCl@lignin activated carbon anode material.

[0009] Lignin is a rich renewable resource, widely present in plant cell walls, especially produced as a byproduct in industries such as papermaking. Due to its wide source and low cost, lignin can reduce the dependence on fossil fuels as a raw material in the production process, thereby reducing production costs. The source of lignin in the present invention is diverse, such as common alkali lignin, eucalyptus lignin, high boiling alcohol lignin, organic solvent lignin, sulfate lignin, enzymolysis lignin, etc. in industrial production, all of which can be used as raw materials for preparation, and those skilled in the art can select the appropriate type according to actual conditions.

[0010] Preferably, in step (1), the lignin comprises at least one of alkali lignin, eucalyptus lignin, high-boiling alcohol lignin, organic solvent lignin, sulfate lignin, and enzymatic lignin.

[0011] Bi precursor and Ag precursor are selected with suitable salts that are soluble and ionized in a solvent environment. Based on this principle and the consideration of raw material sources and costs, Bi precursors can be selected from organic or inorganic salts of bismuth such as bismuth nitrate, bismuth chloride, bismuth sulfate, bismuth acetate, bismuth citrate, bismuth iodide, bismuth bromide, and bismuth phosphate; Ag precursors can be selected from organic or inorganic salts of silver such as silver nitrate, silver acetate, silver phosphate, and silver trifluoroacetate.

[0012] Preferably, in step (1), the Bi precursor includes a bismuth salt and a hydrate thereof, and the bismuth salt includes at least one of bismuth nitrate, bismuth chloride, bismuth sulfate, bismuth acetate, bismuth citrate, bismuth iodide, bismuth bromide, and bismuth phosphate.

[0013] Preferably, in step (1), the Ag precursor includes a silver salt and a hydrate thereof, and the silver salt includes at least one of silver nitrate, silver acetate, silver phosphate and silver trifluoroacetate.

[0014] Based on the selection of Bi precursor, Ag precursor, chloride salt and their solubility characteristics, those skilled in the art can select a suitable solvent and dosage, and some organic solvents can be recycled and reused by rotary evaporation or the like, further reducing production costs.

[0015] Preferably, in step (1), the solvent comprises at least one of tetrahydrofuran, ethanol, ethylene glycol, acetone, dimethyl sulfoxide, dichloromethane and water.

[0016] The ratio of functional materials and lignin in the anode material is appropriately controlled within a suitable range, which can affect the electrochemical performance, structural stability and compatibility with the electrolyte of the anode. The functional materials made from Bi precursors and Ag precursors can provide active sites for electrochemical reactions, while the carbonized structure of lignin can provide mechanical support and electronic conduction paths. If the ratio of functional materials is too high, the anode structure may be unstable, prone to volume expansion and pulverization. If the ratio of functional materials is too low, it may not provide enough active sites, limiting the capacity and efficiency of the battery.

[0017] Preferably, in step (1), the mass ratio of the Bi precursor or the Ag precursor to the lignin is 0.2-2:1.

[0018] Chloride salts are also selected to be suitable salts that are soluble and ionized in a solvent environment, among which sodium chloride and potassium chloride are particularly suitable for the preparation of the present invention due to their wide sources and low costs. Due to the limitation of reaction kinetics, in order to obtain the target AgCl or BiOCl, it is appropriate to add chlorine element slightly higher than the chemical reaction amount during the preparation, so that the reaction of the raw materials is more complete, which is beneficial to improving the quality and use effect of the product.

[0019] Preferably, in step (1), the chloride salt includes at least one of sodium chloride and potassium chloride.

[0020] Preferably, in step (1), the concentration of the aqueous solution of chloride salt is 1-20 mM.

[0021] Preferably, in step (1), the ratio of Bi atoms or Ag atoms in the Bi precursor or Ag precursor to chlorine atoms in the chloride salt is 1-20:1.

[0022] The molecular weight of the dialysis is selected according to the molecular weight of lignin from different sources, so that the lignin is retained and self-assembled in a dialysis device (such as a dialysis bag).

[0023] Preferably, in step (1), the dialyzed molecular weight is 1-12 KD.

[0024] Preferably, in step (1), the temperature of the hydrothermal reaction is 200-500°C, and the reaction time is 2-24 h.

[0025] Preferably, in step (2), the calcination temperature is 400-1000° C. and the calcination time is 0.5-3 h.

[0026] In the second aspect of the present invention, a lignin activated carbon capacitor deionization anode electrode material with good stability, long service life and high adsorption capacity is provided, which is prepared by the method of the first aspect of the present invention.

[0027] In the third aspect of the present invention, there is provided an application of the lignin activated carbon capacitive deionization anode electrode material according to the second aspect of the present invention, specifically, an application as an anode material in capacitive deionization and desalination.

[0028] Preferably, the application method comprises the following steps: mixing the lignin activated carbon capacitive deionization anode electrode material with a conductive agent, a binder, and a solvent to form an anode slurry, which is then coated on the surface of the current collector and dried to form an anode; assembling the components including the anode to obtain a capacitive deionization and desalination device for capacitive deionization and desalination.

[0029] Further preferably, the mass ratio of the lignin activated carbon capacitor deionization anode electrode material, the conductive agent, and the binder is 5-12:1:1.

[0030] Conductive agents, binders, and solvents can use common raw materials in the field, and technicians in this field can choose appropriate combinations according to actual needs. For example, the binder uses common polyvinylidene difluoride (PVDF), the conductive agent uses conductive carbon black that enhances the conductivity of the electrode, and the solvent is usually N-methyl-2-pyrrolidone (NMP). There is no special limitation on the shape of the current collector. Titanium plates, titanium meshes, graphite carbon plates, graphite paper, conductive carbon cloth, etc. are usually used in the field for support and current collection in capacitor deionization.

[0031] The reactions involved in the operation of the lignin activated carbon capacitor deionization anode electrode material are as follows: ; .

[0032] Based on the above technical scheme, the inventive concept and principle of the present invention is to prepare anode materials by combining biomass material lignin with Bi / BiOCl system and Ag / AgCl system that capture chloride ions through redox reaction, so as to save raw material costs to a great extent, improve the high value-added application of lignin, and solve the problem of solid waste treatment in industries such as papermaking. The Bi or Ag precursor material of the present invention adopts a salt that is dissolved in a solvent and ionized, and combines with lignin through the positive and negative charges of the ions. There is no need to synthesize Ag / AgCl or Bi / BiOCl in advance. Compared with other preparation methods, it can obtain an effective and firm load and prevent the agglomeration of materials. The expected Bi@lignin composite material, Ag@lignin composite material, and AgCl@lignin composite material prepared by this method through solvent exchange. The surface of lignin molecules carries a large number of negatively charged functional groups such as alcoholic hydroxyl and phenolic hydroxyl. In the process of solvent exchange from solvent to water, through the self-assembly of molecules, the surface of lignin cluster nanoparticles shows a large number of hydrophilic negatively charged functional groups. Based on this, the design and construction of materials can be carried out to enhance the utilization of higher added value. BiOCl cannot be prepared by solvent exchange at room temperature, so hydrothermal reaction is required to prepare BiOCl@lignin composite materials. Hydrothermal reaction usually refers to a chemical reaction using water or other liquid media under high temperature and high pressure conditions. In this process, water can be in a supercritical state, in which the physical and chemical properties of water will change significantly, allowing some chemical reactions that are difficult to carry out under normal conditions to be carried out. Although water is a commonly used reaction medium, it is not limited to water. Other liquids such as organic solvents can also be used as reaction media as long as these liquids can achieve similar effects under specific temperature and pressure conditions.

[0033] After the required composite material is prepared, it is calcined under an inert atmosphere. In the preparation of Bi@lignin composite materials and Ag@lignin composite materials, metal ions can be effectively reduced under high temperature environment, so that Bi or Ag from the precursor exists in the form of a single substance, reducing the use of other reducing agents. In the present invention, the BiOCl@lignin composite material is prepared by a hydrothermal reaction method, and the Bi precursor, chloride ions and lignin are redox reacted at high temperature to generate the BiOCl@lignin composite material. The presence of lignin limits the large particle growth of BiOCl particles and the agglomeration of nanoparticles, thereby improving the utilization rate and electrochemical cycle life of BiOCl. The high-temperature calcination treatment method increases the conductivity of the composite material, and the gas generated during calcination will generate pores when it is removed from the activated carbon formed by carbonization, thereby increasing the specific surface area of ​​the material, which is beneficial to the transportation and storage of ions in capacitive deionization. The anode material prepared by the method of the present invention has uniform dispersion of active substances, stable composite material structure, and is easy to use. Moreover, by fixing the precursor material on the lignin skeleton in advance, the volume expansion of the material can be better limited, and the attenuation of the desalination capacity can be reduced. It has excellent desalination effect when used as an electrode in hybrid capacitive deionization, dual ion electrochemical deionization, membrane capacitive deionization and other technologies.

[0034] Compared with the prior art, the present invention has the following advantages and beneficial effects: The present invention provides a method for preparing a lignin activated carbon capacitor deionization anode electrode material, which has the advantages of convenient process, low raw material cost, wide source and environmental friendliness.

[0035] The invention provides a lignin activated carbon capacitor deionization anode electrode material, which has the characteristics of good stability, long service life and high adsorption capacity.

[0036] The invention provides an application of a lignin activated carbon capacitive deionization anode electrode material, which has good prospects in the field of capacitive deionization and desalination. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 X-ray diffractometer (XRD) patterns of the Bi@lignin activated carbon anode material and lignin prepared in Example 1; Figure 2 This is a curve obtained by testing the anode prepared in Example 1 using cyclic voltammetry (CV); Figure 3 The constant current charge-discharge curve of the anode prepared in Example 1; Figure 4 The curve obtained by testing the control anode prepared in Example 2 by cyclic voltammetry; Figure 5 It is a structural schematic diagram of a capacitive deionization device; Figure 6 (a) is a conductivity curve of multiple desalination of a capacitive deionization (CDI) device assembled with the anode prepared in Example 1; Figure 6 (b) is the corresponding desalination capacity diagram. DETAILED DESCRIPTION

[0038] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0039] In the following embodiments: X-ray diffractometer model: XRD-6100; Electrochemical workstation model: Shanghai Chenhua CHI760E; Dialysis bag model: 1K MD44.

[0040] Example 1 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of Bi@lignin composite materials: Weigh 0.5 g of ground alkali lignin and 0.5 g of bismuth nitrate into a beaker, add an appropriate amount of tetrahydrofuran, and prepare a 50 mL solution. Stir on a magnetic stirrer until lignin and bismuth nitrate are completely dissolved to obtain a mixed solution; cut a dialysis bag of appropriate length, put the mixed solution into it, and dialyze in deionized water for 24 h; after the dialysis is completed, centrifuge at 3000 rpm, wash with deionized water, and dry at 50 °C to obtain a Bi@lignin composite material; (2) Carbonization of Bi@lignin composites: The Bi@lignin composite material was placed in a tube furnace and carbonized at 800 °C for 2 h under an inert atmosphere to obtain a Bi@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is Bi@lignin activated carbon anode material.

[0041] The prepared Bi@lignin activated carbon anode material was characterized and analyzed by X-ray diffractometer. Figure 1 shown. Figure 1By comparing with the standard cards of lignin and Bi, it can be seen that the Bi@lignin activated carbon anode material shows an obvious Bi diffraction peak, indicating that Bi is successfully loaded in lignin and exists in a single substance after high-temperature reduction.

[0042] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0043] Example 2 In this example, the electrochemical properties of lignin activated carbon capacitive deionization anode electrode materials were studied at room temperature using an electrochemical workstation. Example 1 was used as a representative example of the present invention for testing, and the control sample was lignin activated carbon, the preparation method of which was basically the same as that of Example 1, the only difference being that bismuth nitrate was not added, and the control anode was prepared using the same method. In the test, the Ag / AgCl electrode was the reference electrode, the platinum electrode was the counter electrode, the anode of Example 1 was the working electrode, and a 1 M sodium chloride aqueous solution was used as the electrolyte. The CV test curves of the anode of Example 1 at scan rates of 1 mV / s and 5 mV / s are shown in Figure 2. Figure 2 As shown. Figure 2 It can be seen that a pair of Bi / BiOCl redox peaks appear near -0.75 V and -0.001 V, which is similar to the rectangular CV curve of lignin activated carbon ( Figure 4 ), indicating that the successful loading of Bi in the composite material has improved its electrochemical performance, and the electrochemical performance of Bi@lignin activated carbon anode material is better than that of lignin activated carbon. In addition, at a scan rate of 1 mV / s, the present invention obtains a specific capacitance of up to 207.6 F / g, and still has a specific capacitance of 168.0 F / g at a scan rate of 5 mV / s, proving that the composite material has good rate capability. The loading of Bi is beneficial to its capture and storage of chloride ions, increasing the capacitive deionization and desalination performance. The constant current charge and discharge curve of the anode of Example 1 at a current density of 100 mA / g is shown in the figure. Figure 3 As shown. Figure 3 It can be seen that after multiple constant current charge and discharge cycles, the capacitor still has a stable capacitance, indicating that it has good electrochemical properties.

[0044] Example 3 This example studies the application effect of lignin activated carbon capacitive deionization anode electrode material in capacitive deionization desalination. Figure 5 The capacitive deionization device, the capacitive deionization desalination device specifically includes a capacitive deionization working unit, a peristaltic pump, a circulation pipeline, and a detection system. The sampled salt water is transported into the capacitive deionization working unit by the peristaltic pump, and a working voltage is applied in the working unit. After the ions in the sampled water are captured by the electrode, they flow out from the water outlet to obtain a desalinated aqueous solution. The capacitive deionization working unit is assembled in order from the following materials: a support plate, a gasket, a current collector, an electrode material, a gasket, an anion exchange membrane, a water flow cavity, a cation exchange membrane, a gasket, a cation exchange membrane, an electrode material, a current collector, a gasket, and a support plate. The anode prepared in Example 1 was used as the electrode anode, and the activated carbon electrode was used as the electrode cathode. An anion exchange membrane was added on the anode side, and a cation exchange membrane was added on the cathode side. A 10 mM sodium chloride aqueous solution was transported to the capacitive deionization device by a peristaltic pump, and the solution was transported from the bottom to the top to ensure that there were no bubbles in the device. The electrode clamp of the electrochemical workstation was clamped to the corresponding electrode sheet in the capacitive deionization device. The optimal speed and desalination time of the peristaltic pump were detected by a conductivity meter, and the desalination performance was tested at different voltages, and the cyclic desalination performance was tested at the optimal voltage.

[0045] Figure 6 (a) is the conductivity and time variation diagram of 16 tests, corresponding to Figure 6 (b) is a graph of desalination capacity, and it can be seen that after 16 desalination cycles, the desalination capacity has basically not decreased. There are also several cases of desalination capacity increase during this period. For many electrode materials currently based on Bi / BiOCl redox couple chlorine storage, the capacity loss caused by volume expansion is very serious, especially in the initial cycle, the capacity loss can even reach about 50%. From the test results of this embodiment, it can be seen that the problem of desalination capacity attenuation has been significantly improved, and this is mainly based on the particularity of the materials and preparation methods used in the present invention, which effectively optimizes the defects of the prior art.

[0046] Example 4 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of Bi@lignin composite materials: Weigh 0.5 g of ground lignin and 0.5 g of bismuth nitrate into a beaker, add an appropriate amount of tetrahydrofuran, and prepare a 50 mL solution, stir on a magnetic stirrer, and obtain a mixed solution after the lignin and bismuth nitrate are completely dissolved; cut a dialysis bag of appropriate length, put the mixed solution into it, and dialyze in deionized water for 24 h; after the dialysis is completed, centrifuge at a rate of 3000 rpm, wash with deionized water, and dry at 50 ° C to obtain a Bi@lignin composite material; (2) Carbonization of Bi@lignin composites: The Bi@lignin composite material was placed in a tube furnace and carbonized at 600 °C for 2 h under an inert atmosphere to obtain a Bi@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is Bi@lignin activated carbon anode material.

[0047] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0048] Example 5 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of Bi@lignin composite materials: Weigh 2 g of ground lignin and 0.5 g of bismuth nitrate into a beaker, add an appropriate amount of tetrahydrofuran, and prepare a 50 mL solution. Stir on a magnetic stirrer until the lignin and bismuth nitrate are completely dissolved to obtain a mixed solution; cut a dialysis bag of appropriate length, put the mixed solution into it, and dialyze in deionized water for 24 h; after the dialysis is completed, centrifuge at 3000 rpm, wash with deionized water, and dry at 50 °C to obtain a Bi@lignin composite material; (2) Carbonization of Bi@lignin composites: The Bi@lignin composite material was placed in a tube furnace and carbonized at 900 °C for 2 h under an inert atmosphere to obtain a Bi@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is Bi@lignin activated carbon anode material.

[0049] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0050] Example 6 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of Bi@lignin composite materials: Weigh 0.5 g of high-boiling alcohol lignin and 0.5 g of bismuth nitrate into a beaker, add an appropriate amount of tetrahydrofuran, and prepare a 50 mL solution, stir on a magnetic stirrer, and obtain a mixed solution after the high-boiling alcohol lignin and bismuth nitrate are completely dissolved; cut a dialysis bag of appropriate length, put the above mixed solution into it, and dialyze in deionized water for 24 h; after the dialysis is completed, centrifuge at a rate of 3000 rpm, wash with deionized water, and dry at 50 ° C to obtain a Bi@lignin composite material; (2) Carbonization of Bi@lignin composites: The Bi@lignin composite material was placed in a tube furnace and carbonized at 900 °C for 2 h under an inert atmosphere to obtain a Bi@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is Bi@lignin activated carbon anode material.

[0051] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0052] Example 7 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of Bi@lignin composite materials: Weigh 0.5 g of enzymatically hydrolyzed lignin and 0.5 g of bismuth nitrate into a beaker, add an appropriate amount of tetrahydrofuran, and prepare a 50 mL solution, stir on a magnetic stirrer, and obtain a mixed solution after the enzymatically hydrolyzed lignin and bismuth nitrate are completely dissolved; cut a dialysis bag of appropriate length, put the above mixed solution into it, and dialyze in deionized water for 24 h; after the dialysis is completed, centrifuge at a rate of 3000 rpm, wash with deionized water, and dry at 50 °C to obtain a Bi@lignin composite material; (2) Carbonization of Bi@lignin composites: The Bi@lignin composite material was placed in a tube furnace and carbonized at 800 °C for 2 h under an inert atmosphere to obtain a Bi@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is Bi@lignin activated carbon anode material.

[0053] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0054] Example 8 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of Bi@lignin composite materials: Weigh 0.5 g of ground lignin and 0.5 g of bismuth acetate into a beaker, add an appropriate amount of tetrahydrofuran, and prepare a 50 mL solution, stir on a magnetic stirrer, and obtain a mixed solution after lignin and bismuth acetate are completely dissolved; cut a dialysis bag of appropriate length, put the mixed solution into it, and dialyze in deionized water for 24 h; after the dialysis is completed, centrifuge at 3000 rpm, wash with deionized water, and dry at 50 °C to obtain a Bi@lignin composite material; (2) Carbonization of Bi@lignin composites: The Bi@lignin composite material was placed in a tube furnace and carbonized at 800 °C for 2 h under an inert atmosphere to obtain a Bi@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is Bi@lignin activated carbon anode material.

[0055] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0056] Example 9 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of Bi@lignin composite materials: Weigh 0.5 g of ground lignin and 0.5 g of bismuth phosphate into a beaker, add an appropriate amount of tetrahydrofuran, and prepare a 50 mL solution, stir on a magnetic stirrer, and obtain a mixed solution after lignin and bismuth phosphate are completely dissolved; cut a dialysis bag of appropriate length, put the mixed solution into it, and dialyze in deionized water for 24 h; after the dialysis is completed, centrifuge at 3000 rpm, wash with deionized water, and dry at 50 ° C to obtain a Bi@lignin composite material; (2) Carbonization of Bi@lignin composites: The Bi@lignin composite material was placed in a tube furnace and carbonized at 800 °C for 2 h under an inert atmosphere to obtain a Bi@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is Bi@lignin activated carbon anode material.

[0057] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0058] Example 10 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of Ag@lignin composite materials: Weigh 0.5 g of ground lignin and 0.5 g of silver nitrate into a beaker, add an appropriate amount of tetrahydrofuran, and prepare a 50 mL solution. Stir on a magnetic stirrer until the lignin and silver nitrate are completely dissolved to obtain a mixed solution; cut a dialysis bag of appropriate length, put the mixed solution into it, and dialyze in deionized water for 24 h; after the dialysis is completed, centrifuge at 3000 rpm, wash with deionized water, and dry at 50 °C to obtain the Ag@lignin composite material; (2) Carbonization of Ag@lignin composites: The Ag@lignin composite material was placed in a tube furnace and carbonized at 800 °C for 2 h under an inert atmosphere to obtain an Ag@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is Ag@lignin activated carbon anode material.

[0059] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0060] Embodiment 11 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of Ag@lignin composite materials: Weigh 0.5 g of ground lignin and 0.5 g of silver trifluoroacetate into a beaker, add an appropriate amount of tetrahydrofuran, and prepare a 50 mL solution. Stir on a magnetic stirrer until the lignin and silver trifluoroacetate are completely dissolved to obtain a mixed solution; cut a dialysis bag of appropriate length, put the mixed solution into it, and dialyze in deionized water for 24 h; after the dialysis is completed, centrifuge at 3000 rpm, wash with deionized water, and dry at 50 °C to obtain an Ag@lignin composite material; (2) Carbonization of Ag@lignin composites: The Ag@lignin composite material was placed in a tube furnace and carbonized at 800 °C for 2 h under an inert atmosphere to obtain an Ag@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is Ag@lignin activated carbon anode material.

[0061] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0062] Example 12 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of Bi@lignin composite materials: Weigh 0.5 g of ground lignin and 0.5 g of bismuth nitrate into a beaker, add an appropriate amount of acetone, and prepare a 50 mL solution. Stir on a magnetic stirrer until the lignin and bismuth nitrate are completely dissolved to obtain a mixed solution; cut a dialysis bag of appropriate length, put the mixed solution into it, and dialyze in deionized water for 24 h; after the dialysis is completed, centrifuge at 3000 rpm, wash with deionized water, and dry at 50 °C to obtain a Bi@lignin composite material; (2) Carbonization of Bi@lignin composites: The Bi@lignin composite material was placed in a tube furnace and carbonized at 800 °C for 2 h under an inert atmosphere to obtain a Bi@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is Bi@lignin activated carbon anode material.

[0063] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0064] Embodiment 13 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of Ag@lignin composite materials: Weigh 0.5 g of ground lignin and 0.5 g of silver nitrate into a beaker, add an appropriate amount of ethanol, and prepare a 50 mL solution. Stir on a magnetic stirrer until the lignin and silver nitrate are completely dissolved to obtain a mixed solution; cut a dialysis bag of appropriate length, put the mixed solution into it, and dialyze in deionized water for 24 h; after the dialysis is completed, centrifuge at 3000 rpm, wash with deionized water, and dry at 50 °C to obtain the Ag@lignin composite material; (2) Carbonization of Ag@lignin composites: The Ag@lignin composite material was placed in a tube furnace and carbonized at 800 °C for 2 h under an inert atmosphere to obtain an Ag@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is Ag@lignin activated carbon anode material.

[0065] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0066] Embodiment 14 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of BiOCl@lignin composite materials: 0.5 g of bismuth nitrate pentahydrate and 0.09 g of potassium chloride were dissolved in 10 mL of ethylene glycol, 0.1 g of lignin and 50 mL of ethanol were added to the mixed solution, stirred and dissolved, and then transferred to a hydrothermal reactor and reacted at 160 °C for 24 h. The prepared solid particles were collected, filtered, washed with distilled water, and dried at 60 °C to obtain BiOCl@lignin composite materials; (2) Carbonization of BiOCl@lignin composites: The BiOCl@lignin composite material was placed in a tube furnace and carbonized at 500 °C for 2 h under an inert atmosphere to obtain the BiOCl@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is BiOCl@lignin activated carbon anode material.

[0067] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0068] Embodiment 15 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of BiOCl@lignin composite materials: 1.5 g of bismuth nitrate pentahydrate and 0.25 g of potassium chloride were dissolved in 10 mL of ethylene glycol, 0.2 g of lignin and 50 mL of ethanol were added to the mixed solution, stirred and dissolved, and then transferred to a hydrothermal reactor and reacted at 160 °C for 24 h. The prepared solid particles were collected, filtered, washed with distilled water, and dried at 60 °C to obtain BiOCl@lignin composite materials; (2) Carbonization of BiOCl@lignin composites: The BiOCl@lignin composite material was placed in a tube furnace and carbonized at 500 °C for 2 h under an inert atmosphere to obtain the BiOCl@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is BiOCl@lignin activated carbon anode material.

[0069] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0070] Example 16 The preparation method of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: (1) Preparation of AgCl@lignin composite materials: Weigh 0.5 g of ground lignin and 0.5 g of silver nitrate into a beaker, add an appropriate amount of tetrahydrofuran, and prepare a 50 mL solution, stir on a magnetic stirrer, and obtain a mixed solution after the lignin and silver nitrate are completely dissolved; cut a dialysis bag of appropriate length, put the mixed solution into it, and dialyze it in an aqueous solution containing 10 mmol sodium chloride for 24 h; after the dialysis is completed, centrifuge at a rate of 3000 rpm, wash with deionized water, and dry at 50 °C to obtain AgCl@lignin composite material; (2) Carbonization of AgCl@lignin composites: The AgCl@lignin composite material was placed in a tube furnace and carbonized at 400 °C for 2 h under an inert atmosphere to obtain an AgCl@lignin activated carbon anode material. (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material of this embodiment is AgCl@lignin activated carbon anode material.

[0071] This embodiment also provides an anode made of lignin activated carbon capacitor deionization anode electrode material, the steps are as follows: The lignin activated carbon capacitor deionization anode electrode material, conductive carbon powder and PVDF were mixed in an agate crucible in a ratio of 8:1:1, NMP was added dropwise and ground evenly, and after grinding evenly, it was smeared on the weighed and recorded graphite paper, placed in a blower dryer for drying, weighed and recorded after drying, to obtain the prepared anode.

[0072] In summary, the lignin used in the present invention is a renewable biomass material, containing a large amount of phenolic hydroxyl and alcoholic hydroxyl groups with green environmental protection, low cost, easy to use characteristics, and lignin microspheres are formed by a simple, highly operable preparation method. Lignin microspheres increase the specific surface area of ​​the material, and a large number of negatively charged groups are distributed on its surface, which can interact with metal ions, so that Ag and Bi with electrochemical capture of chloride ions are loaded in the microspheres, which can effectively suppress the huge volume expansion brought by Ag and Bi when electrochemically capturing chloride ions, and enhance its adsorption capacity as anode. Different from other MOF-derived carbons, the present invention selects lignin as a carbon material suitable for actual production applications, compared to other materials, such as aerogels, flexible films composed of two-dimensional nanomaterials, etc., its mechanical strength is greater, stability is better, and relative service life is longer. Lignin belongs to biomacromolecules, and metal elements are firmly locked by charge interaction, and self-assembly can be performed by hydrogen bonds or π bonds, so that the whole composite material structure is more firm and effective, and anode electrode materials with larger capacity and faster adsorption rate are obtained, which can more effectively avoid the adsorption capacity loss caused by volume expansion, and increase the service life of the electrode. The lignin activated carbon capacitive deionization anode electrode material prepared by the present invention has a wide range of uses, has good applicability in conventional capacitive deionization, membrane capacitive deionization, dual-ion electrochemical deionization and other capacitive deionization devices based on electrochemical ion capture, and has broad application prospects.

[0073] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing a lignin activated carbon capacitor deionization anode electrode material, characterized in that: The steps include: (1) Preparation of corresponding composite materials based on the components of lignin activated carbon capacitor deionization anode electrode materials: a. Mixing lignin, Bi precursor or Ag precursor with a solvent, dialyzing the resulting mixed solution in water to complete solvent exchange, and recovering the corresponding Bi@lignin composite material or Ag@lignin composite material; b. Mixing lignin, Ag precursor and solvent, dialyzing the resulting mixture in an aqueous solution of chloride salt to complete solvent exchange, and recovering the AgCl@lignin composite material; c. Mixing lignin, Bi precursor, chloride salt and solvent, and then performing a hydrothermal reaction; after the hydrothermal reaction is completed, recovering to obtain the BiOCl@lignin composite material; The Bi precursor, the Ag precursor, and the chloride salt are salts that are dissolved in a solvent and ionized; (2) Carbonization of composite materials: The Bi@lignin composite material, the Ag@lignin composite material, the AgCl@lignin composite material, and the BiOCl@lignin composite material are respectively subjected to calcination treatment in an inert atmosphere to complete carbonization, and Bi@lignin activated carbon anode material, BiOCl@lignin activated carbon anode material, Ag@lignin activated carbon anode material, and AgCl@lignin activated carbon anode material are obtained accordingly; (3) Obtaining lignin activated carbon capacitor deionization anode electrode material: The lignin activated carbon capacitor deionization anode electrode material includes at least one of Bi@lignin activated carbon anode material, BiOCl@lignin activated carbon anode material, Ag@lignin activated carbon anode material, and AgCl@lignin activated carbon anode material.

2. The method for preparing the lignin activated carbon capacitor deionization anode electrode material according to claim 1, characterized in that: In the step (1), the lignin includes at least one of alkali lignin, eucalyptus lignin, high-boiling alcohol lignin, organic solvent lignin, sulfate lignin, and enzymatic lignin; the Bi precursor includes a bismuth salt and a hydrate thereof, and the bismuth salt includes at least one of bismuth nitrate, bismuth chloride, bismuth sulfate, bismuth acetate, bismuth citrate, bismuth iodide, bismuth bromide, and bismuth phosphate; the Ag precursor includes a silver salt and a hydrate thereof, and the silver salt includes at least one of silver nitrate, silver acetate, silver phosphate, and silver trifluoroacetate; and the mass ratio of the Bi precursor or the Ag precursor to the lignin is 0.2-2:

1.

3. The method for preparing the lignin activated carbon capacitor deionization anode electrode material according to claim 1, characterized in that: In the step (1), the solvent includes at least one of tetrahydrofuran, ethanol, ethylene glycol, acetone, dimethyl sulfoxide, dichloromethane and water.

4. The method for preparing the lignin activated carbon capacitor deionization anode electrode material according to claim 1, characterized in that: In the step (1), the chloride salt includes at least one of sodium chloride and potassium chloride; the concentration of the chloride salt aqueous solution is 1-20 mM; and the ratio of Bi atoms or Ag atoms in the Bi precursor or the Ag precursor to chlorine atoms in the chloride salt is 1-20:

1.

5. The method for preparing the lignin activated carbon capacitor deionization anode electrode material according to claim 1, characterized in that: In the step (1), the dialyzed molecular weight is 1-12 KD.

6. The method for preparing the lignin activated carbon capacitor deionization anode electrode material according to claim 1, characterized in that: In the step (1), the temperature of the hydrothermal reaction is 200-500°C, and the reaction time is 2-24 h.

7. The method for preparing the lignin activated carbon capacitor deionization anode electrode material according to claim 1, characterized in that: In the step (2), the calcination temperature is 400-1000°C and the calcination time is 0.5-3 h.

8. A lignin activated carbon capacitor deionization anode electrode material, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 7.

9. An application of the lignin activated carbon capacitor deionization anode electrode material as claimed in claim 8, characterized in that: Application as anode material in capacitive deionization and desalination.

10. The use of the lignin activated carbon capacitor deionization anode electrode material according to claim 9, characterized in that: The application method includes the following steps: mixing lignin activated carbon capacitive deionization anode electrode material with a conductive agent, a binder, and a solvent to form an anode slurry, which is then coated on the surface of a current collector and dried to form an anode; assembling the components including the anode to obtain a capacitive deionization and desalination device for capacitive deionization and desalination.

Citation Information

Patent Citations

  • Preparation method of lignin carbon / bismuth oxide composite material and pseudocapacitance performance of lignin carbon / bismuth oxide composite material

    CN112479178A

  • Composite electrode material of graphene-based ultra-small oxyhalogen bismuth nanoparticles and preparation method thereof

    CN113800560A

  • Reduction modified lignin-based activated carbon for supercapacitor electrode material and preparation method and application of reduction modified lignin-based activated carbon

    CN117334487A

  • Preparation method of lignin-based carbon bifunctional composite material and application of lignin-based carbon bifunctional composite material in heavy metal removal and organic dye degradation

    CN117563555A

  • Preparation method and application of lignin carbon quantum dot modified bismuth vanadate nanocomposite

    CN117983204A

Cited By

  • Silicon-rich biomass electrode material, preparation method thereof and application of silicon-rich biomass electrode material in adjusting pH of papermaking wastewater