Spherical-like micro-nano copper powder and preparation method and application thereof

CN118905235APending Publication Date: 2024-11-08SHENZHEN HASHEN TECHNOLOGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410974385.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing preparation methods for micro-nano copper powder, particle size control is difficult, particle aggregation is serious, environmental and safety problems are prominent, and chemical stability is poor, which affects the performance and application of conductive inks.

Method used

The two-stage reaction and rapid cooling method are adopted to form copper particles by rapid cooling after the first stage of reaction. The second stage of reaction is carried out at a lower temperature, using ascorbic acid and gelatin as reducing agents, and combining copper formate as nucleation agents , control particle size and morphology to avoid agglomeration.

Benefits of technology

The copper powder particle size is small, the particle size distribution is uniform, and there is no agglomeration phenomenon, which improves the performance and stability of conductive inks, and reduces production costs and environmental impacts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905235A_ABST
    Figure CN118905235A_ABST
Patent Text Reader

Abstract

The invention discloses sphere-like micro-nano copper powder as well as a preparation method and application thereof, and relates to the technical field of metal materials. The preparation method of the spherical micro-nano copper powder comprises the following steps: mixing a reducing base solution and a copper salt nucleation solution, and reacting at 50-90 DEG C for 0.5-4 minutes; rapidly cooling to 20 DEG C to 45 DEG C within 3 to 15 minutes; a copper salt growth solution is injected, and a reaction is conducted for 6-20 min; and carrying out solid-liquid separation, washing and drying to obtain the sphere-like micro-nano copper powder. The sphere-like micro-nano copper powder is prepared in a two-stage reaction and rapid cooling mode, after the first-stage reaction is finished, rapid cooling is carried out, the nucleation and growth processes involved in the copper particle forming process can be effectively separated, and then the effects of limiting the particle size and the agglomeration phenomenon and keeping excellent particle size distribution are achieved. The prepared sphere-like micro-nano copper powder can be widely applied to preparation of conductive ink.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal materials, and in particular to a quasi-spherical micro-nano copper powder and a preparation method and application thereof. Background Art

[0002] Conductive ink is a material that is widely used in the electronics manufacturing industry, especially in printed circuit boards, flexible circuits, touch screen technology and wearable electronic devices. It can form conductive paths on various substrates and is a key technology for realizing thin, short and flexible electronic products. In the preparation of conductive ink, the selection of the conductive phase (conductive particles) is crucial because it directly determines the conductivity, stability and final application performance of the ink. The conductive particles must have excellent electrical properties and should be kept as stable as possible during the use of the ink to avoid oxidation and other changes.

[0003] Among the common conductive phases, gold, silver, and copper are common options. Although nano-gold powder and nano-silver powder have advantages in conductivity and stability, the expensive raw material costs of gold and silver greatly limit mass production. In addition, the electromigration problem of silver will also affect the reliability of subsequent applications. Although the electrical conductivity of copper is slightly lower than that of gold and silver, it is sufficient to meet the needs of most conductive inks. In addition, copper is widely present in nature, its price is much lower than that of gold and silver, and it has a certain ability to resist electromigration. It is regarded as a potential substitute for nano-gold powder and nano-silver powder.

[0004] The main methods for preparing micro-nano copper powder at this stage include: physical methods (spheroidal graphite method, vapor deposition method) and chemical methods (microemulsion method, liquid phase reduction method). Among them, the liquid phase reduction method is favored in actual production due to its controllable particle size, low cost, and easy collection.

[0005] The liquid phase reduction method is based on the process of reducing a metal ion solution into metal powder through a chemical reducing agent. For the preparation of micro-nano copper powder, the main reducing agents at this stage include: hydrazine hydrate, sodium borohydride, formaldehyde, ascorbic acid, etc. The preparation process includes the dissolution of metal salts, the redox reaction of metal precursors and reducing agents, and the post-treatment of metal particles (centrifugation, filtration, drying, etc.). Most of the existing liquid phase reduction technologies for micro-nano copper powders at home and abroad directly mix the metal precursor solution with the reducing solution in one step. This preparation scheme has some shortcomings:

[0006] 1. Difficulty in particle size control: Controlling the particle size and morphology of copper powder is the main challenge. Slight changes in reaction conditions will have a significant impact on the microstructure and particle size distribution of the final product. Too uneven particle size distribution will also directly affect the uniformity and conductivity of the conductive ink.

[0007] 2. Particle aggregation: Due to the large specific surface area and high activity of micro-nano particles, they tend to spontaneously aggregate during the preparation process. This phenomenon directly affects the stability and dispersibility of copper powder, thereby reducing the conductivity of conductive ink. The aggregation problem needs to be solved by introducing surfactants or dispersants.

[0008] 3. Environmental and safety issues: Although some strong reducing agents can prepare micro-nano copper powder with very small particle size, they are potentially harmful to the environment and operators, such as formaldehyde, hydrazine hydrate and sodium borohydride. They are dangerous and may cause safety accidents if not handled properly.

[0009] 4. Chemical stability and oxidation issues: Copper powder is very easy to oxidize in the air, and the conductivity of the oxidized copper powder will decrease, which not only increases the manufacturing cost (such as operating in an inert gas environment), but also limits the long-term storage and transportation of copper powder.

[0010] In view of this, the present invention is proposed. Summary of the invention

[0011] The object of the present invention is to provide a spherical micro-nano copper powder and a preparation method and application thereof, so as to improve at least one of the above-mentioned deficiencies.

[0012] The present invention is achieved in that:

[0013] In a first aspect, the present invention provides a method for preparing spherical micro-nano copper powder, comprising:

[0014] The reducing base liquid and the copper salt nucleation liquid are mixed, and the first stage reaction is carried out at 50°C-90°C for 0.5min-4min to obtain a first mixed liquid; wherein the reducing base liquid comprises 0.02g / ml-0.50g / ml of ascorbic acid and 0.01g / ml-0.10g / ml of gelatin, and the copper salt nucleation liquid comprises 0.02g / ml-0.25g / ml of copper formate;

[0015] Rapidly cool the first mixed solution to 20°C-45°C within 3-15 minutes;

[0016] Injecting the copper salt growth solution into the cooled first mixed solution to carry out a second stage reaction, the reaction time is 6 min-20 min; obtaining a second mixed solution; wherein the copper salt growth solution comprises 0.003 g / ml-0.018 g / ml of copper formate;

[0017] The second mixed liquid is separated into solid and liquid, washed and dried to obtain spherical micro-nano copper powder.

[0018] In an optional embodiment, before the reducing base liquid and the copper salt nucleation liquid are mixed, the copper salt nucleation liquid and the reducing base liquid are heated and kept warm respectively;

[0019] Preferably, the holding temperature of the copper salt nucleation solution is 43°C-75°C;

[0020] Preferably, the insulation temperature of the reducing base solution is 50°C-90°C;

[0021] Preferably, the mixing method of the reducing base liquid and the copper salt nucleation liquid comprises adding the copper salt nucleation liquid into the reducing base liquid.

[0022] In an optional embodiment, the copper formate in the copper salt nucleation solution accounts for 80%-90% of the total mass of the copper formate in the copper salt nucleation solution and the copper salt growth solution.

[0023] In an optional embodiment, the copper salt nucleation solution further includes PVP 0.02 g / ml-0.20 g / ml, and the copper salt growth solution further includes PVP 0.001 g / ml-0.20 g / ml;

[0024] Preferably, the copper salt nucleation solution further includes 0.02 g / ml-0.30 g / ml of sodium citrate, and the copper salt growth solution further includes 0.01 g / ml-0.06 g / ml of sodium citrate.

[0025] In an optional embodiment, the solvents of the reducing base solution and the copper salt growth solution are both water, and the solvent of the copper salt nucleation solution is ethylene glycol or a mixture of ethylene glycol and water in a volume ratio of 1:(1-6).

[0026] In an optional embodiment, the copper salt growth solution is injected into the first mixed solution through an injection pump, the injection speed is 250ml / h-1200ml / h, and the system temperature is maintained at 20°C-45°C after injection;

[0027] In an optional embodiment, the first-stage reaction and the second-stage reaction are both carried out under stirring, and the stirring speed is 300r / min-1200r / min.

[0028] In an optional embodiment, the solid-liquid separation comprises centrifugation, filtration or filter pressing;

[0029] Preferably, the centrifugal speed is 1000r / min-4000r / min;

[0030] Preferably, the centrifugation is performed 2-3 times, each time for 1 min to 2 min.

[0031] In an optional embodiment, the drying comprises drying in a vacuum drying oven at 40° C.-55° C. for 10 min-2 h.

[0032] In a second aspect, the present invention provides a quasi-spherical micro-nano copper powder, which is prepared by the preparation method of the quasi-spherical micro-nano copper powder as described in any one of the aforementioned embodiments;

[0033] Preferably, the particle size of the quasi-spherical micro-nano copper powder is 100nm-400nm.

[0034] In a third aspect, the present invention provides an application of spherical micro-nano copper powder in preparing conductive ink.

[0035] The present invention has the following beneficial effects:

[0036] The preparation method of quasi-spherical micro-nano copper powder provided by the present invention is to prepare quasi-spherical micro-nano copper powder by two-stage reaction and rapid cooling. After the first stage reaction is completed, rapid cooling can effectively separate the nucleation and growth processes involved in the copper particle formation process, thereby achieving the effect of limiting the particle size and agglomeration phenomenon and maintaining excellent particle size distribution. At the same time, the temperature of the second stage reaction is lower than the temperature of the first stage reaction, and the reaction time is longer than the time of the first stage reaction, so that the reaction system reacts for a short time under high temperature conditions in the first stage reaction, and reacts for a longer time at a lower temperature in the second stage reaction, so that a large number of copper crystal nuclei can be "explosively" formed in a short time. The copper formate content of the copper salt nucleation liquid and the copper salt growth liquid is quite different, which can achieve the purpose of "large nucleation + slow growth". The copper powder prepared by the preparation method of quasi-spherical micro-nano copper powder provided by the present invention has a small particle size, a uniform particle size distribution and no obvious agglomeration phenomenon. It can be widely used in the preparation of conductive ink. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0038] Figure 1 This is a SEM image of the spherical micro-nano copper powder provided in Example 1 of the present invention;

[0039] Figure 2 This is a SEM image of the spherical micro-nano copper powder provided in Example 2 of the present invention;

[0040] Figure 3 This is a SEM image of the spherical micro-nano copper powder provided in Example 3 of the present invention;

[0041] Figure 4 This is a SEM image of the spherical micro-nano copper powder provided in Example 4 of the present invention;

[0042] Figure 5 The XRD pattern of the spherical micro-nano copper powder provided in Example 4 of the present invention;

[0043] Figure 6 This is a SEM image of the spherical micro-nano copper powder provided in Example 5 of the present invention;

[0044] Figure 7 This is a SEM image of the spherical micro-nano copper powder provided in Example 6 of the present invention;

[0045] Figure 8 This is a SEM image of the spherical micro-nano copper powder provided in Example 7 of the present invention at a scale of 500 nm;

[0046] Fig. 9 This is a SEM image of the spherical micro-nano copper powder provided in Example 7 of the present invention at a scale of 1 μm;

[0047] Fig.10 This is a SEM image of the spherical micro-nano copper powder provided in Example 7 of the present invention at a scale of 2 μm;

[0048] Fig.11 This is a SEM image of the spherical micro-nano copper powder provided in Example 8 of the present invention;

[0049] Fig.12 This is a SEM image of the spherical micro-nano copper powder provided in Example 9 of the present invention;

[0050] Fig.13 This is a SEM image of the spherical micro-nano copper powder provided in Example 10 of the present invention;

[0051] Fig.14 This is a SEM image of the spherical micro-nano copper powder provided in Example 11 of the present invention;

[0052] Fig.15 This is a SEM image of the copper powder provided in Comparative Example 1 of the present invention;

[0053] Fig.16 This is a SEM image of the copper powder provided in Comparative Example 2 of the present invention;

[0054] Fig.17 This is a SEM image of the copper powder provided in Comparative Example 3 of the present invention;

[0055] Fig.18 This is a SEM image of the copper powder provided in Comparative Example 4 of the present invention;

[0056] Fig.19This is a SEM image of the copper powder provided in Comparative Example 5 of the present invention;

[0057] Fig. 20 This is a SEM image of the copper powder provided in Comparative Example 6 of the present invention;

[0058] Fig.21 This is a SEM image of the copper powder provided in Comparative Example 7 of the present invention;

[0059] Fig. 22 This is a SEM image of the copper powder provided in Comparative Example 8 of the present invention;

[0060] Fig.23 This is a SEM image of the copper powder provided in Comparative Example 9 of the present invention. DETAILED DESCRIPTION

[0061] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0062] The present invention provides a quasi-spherical micro-nano copper powder, and a preparation method thereof comprises the following steps:

[0063] The reducing base liquid and the copper salt nucleation liquid are mixed, and the first stage reaction is carried out at 50°C-90°C for 0.5min-4min to obtain a first mixed liquid; wherein the reducing base liquid includes 0.02g / ml-0.50g / ml of ascorbic acid and 0.01g / ml-0.10g / ml of gelatin, and the copper salt nucleation liquid includes 0.02g / ml-0.25g / ml of copper formate;

[0064] Rapidly cool the first mixed solution to 20°C-45°C within 3-15 minutes;

[0065] Inject the copper salt growth solution into the cooled first mixed solution to carry out a second stage reaction, the reaction time is 6min-20min; obtain a second mixed solution; wherein the copper salt growth solution includes 0.003g / ml-0.018g / ml of copper formate;

[0066] The second mixed liquid is separated into solid and liquid, washed and dried to obtain spherical micro-nano copper powder.

[0067] In the present invention, spherical micro-nano copper powder is prepared by a two-stage reaction and rapid cooling. After the first stage reaction is completed, rapid cooling can effectively separate the nucleation and growth processes involved in the formation of copper particles, thereby achieving the effect of limiting particle size and agglomeration and maintaining excellent particle size distribution.

[0068] Specifically, the present invention comprises the following steps:

[0069] S1. Prepare reducing base solution, copper salt nucleation solution and copper salt growth solution.

[0070] The reducing base liquid includes 0.02g / ml-0.50g / ml of ascorbic acid and 0.01g / ml-0.10g / ml of gelatin, and the solvent of the reducing base liquid is water. In some embodiments, a certain amount of sodium citrate can also be added to the reducing base liquid.

[0071] Ascorbic acid (vitamin C) is a non-toxic and harmless mild reducing agent, and no gas is generated during the production process, which is very suitable for mass production of micro-nano copper powder for conductive ink, but its reducing ability is slightly insufficient compared to strong reducing agents such as hydrazine hydrate, sodium borohydride, and formaldehyde, and there are certain challenges in preparing micro-nano copper powder. However, although it has been proved that the above-mentioned reducing agents with strong reducing ability can prepare micro-nano copper powder with uniform particle size distribution, there are strong toxicity and volatility in the reaction process, which greatly reduces its application prospects in actual production. In the present invention, by compounding ascorbic acid with gelatin, it is conducive to improving the dispersibility in the reduction base liquid, so that it is immediately in a dispersed system when it is convenient to react later.

[0072] The copper salt nucleation solution includes 0.02g / ml-0.25g / ml of copper formate, and the copper salt growth solution includes 0.003g / ml-0.018g / ml of copper formate. The copper formate in the copper salt nucleation solution accounts for 80%-90% of the total mass of the copper formate in the copper salt nucleation solution and the copper salt growth solution.

[0073] In the present invention, the content and concentration of copper formate in the copper salt nucleation liquid are relatively high, and when it is subsequently mixed with the reducing base liquid, it can react relatively quickly at high temperature, and a large number of copper crystal nuclei can be "explosively" formed in a short time. The difference in the content of copper formate in the copper salt nucleation liquid and the copper salt growth liquid is large, which can achieve the purpose of "large-scale nucleation + slow growth". When the ratio of the two is reduced, such as 7:3 and 6:4, the size of the obtained copper particles will be greatly increased, which will have an adverse effect on the preparation effect.

[0074] In other embodiments of the present invention, the copper salt nucleation solution also includes PVP 0.02-0.20 g / ml, and the copper salt growth solution also includes PVP 0.001-0.20 g / ml. PVP can be adsorbed on the surface of copper particles, restricting the agglomeration behavior of copper crystal nuclei and improving the stability and dispersibility of copper powder.

[0075] In other embodiments of the present invention, the copper salt nucleation solution further includes 0.02-0.30 g / ml of sodium citrate, and the copper salt growth solution further includes 0.01-0.06 g / ml of sodium citrate. Sodium citrate can form a stable chelate complex with copper ions, which has the effect of regulating the nucleation reaction rate and buffering the pH value of the reaction system.

[0076] The copper salt nucleation liquid and the reducing base liquid are heated and kept warm; preferably, the keeping temperature of the copper salt nucleation liquid is 43°C-75°C; the keeping temperature of the reducing base liquid is 50°C-90°C.

[0077] Among them, since the gelatin in the reducing base liquid is difficult to dissolve at room temperature, the reducing base liquid is heated in the present invention, and the gelatin gradually dissolves during the heating process to achieve uniform dispersion and dissolution. The insulation temperature of the reducing base liquid in the present invention is designed to be the same as the temperature of the subsequent reaction, so that the reaction temperature can be quickly reached after the copper salt nucleation liquid is added to react.

[0078] In the present invention, the copper salt nucleation liquid is kept warm at a temperature slightly lower than the reaction temperature, so that the temperature of the reaction system will not be greatly reduced when the copper salt nucleation liquid is added to the reducing base liquid. At the same time, the reaction between the reducing base liquid and the copper salt nucleation liquid is an exothermic reaction, which can be heated during the mixing process to quickly achieve the reaction problem. In the present invention, the reducing base liquid and the copper salt nucleation liquid are heated and kept warm to avoid the situation where the temperature difference is too large when the copper salt nucleation liquid at room temperature contacts the reducing base liquid at high temperature.

[0079] The solvent of the copper salt growth liquid is water, and the solvent of the copper salt nucleation liquid is ethylene glycol or a mixture of ethylene glycol and water in a volume ratio of 1:(1-6). In the present invention, ethylene glycol is selected as the solvent of the copper salt nucleation liquid. Ethylene glycol has a certain viscosity, which can reduce the movement and growth trend of copper particles, avoid the copper powder from growing immediately after nucleation, and is conducive to limiting the particle size and size of the copper powder.

[0080] In addition, it should be noted that in the process of preparing the solution in the present invention, stirring and mixing are carried out under ultrasonic conditions, wherein the stirring speed is about 300r / min-1200r / min, and a certain stirring speed needs to be maintained during the insulation process, and the stirring speed can also be 300r / min-1200r / min.

[0081] S2, first stage reaction.

[0082] The reducing base liquid and the copper salt nucleation liquid are mixed, and the first stage reaction is carried out at 50° C.-90° C. for 0.5 min-4 min to obtain a first mixed solution.

[0083] The mixing method of the reducing base liquid and the copper salt nucleation liquid includes adding the copper salt nucleation liquid into the reducing base liquid. The first stage reaction is carried out under stirring, and the stirring speed is 300r / min-1200r / min.

[0084] The reaction time of the first stage reaction should not be too long, because when the temperature is high, the movement rate of the copper particles is extremely high. If the reaction time is set too long, the already generated crystal nuclei will enter the growth stage prematurely.

[0085] S3. Rapid cooling.

[0086] Rapidly cool the first mixed solution to 20°C-45°C within 3-15 minutes; the rapid cooling in the present invention is to "substantially limit" the growth and agglomeration tendency of a large number of copper nuclei generated in the previous stage. This allows the copper nuclei to be evenly dispersed in the system and greatly reduces the driving force for their continued growth and agglomeration. This is a critical stage for limiting the size of copper particles. There are many ways to rapidly cool, including but not limited to freezing in the freezer layer of a refrigerator, ice bath cooling, liquid nitrogen cooling, etc.

[0087] S4, second stage reaction.

[0088] The copper salt growth liquid is injected into the first mixed liquid through an injection pump at an injection speed of 250-1200 ml / h. After injection, the system temperature is maintained at 20°C-45°C for the second stage reaction, and the reaction time is 6-20 minutes to obtain the second mixed liquid. The second stage reaction is carried out under stirring at a stirring speed of 300r / min-1200r / min.

[0089] In the present invention, the temperature of the second stage reaction is lowered, which can slow down the growth rate and avoid excessive growth, resulting in excessively large particle size.

[0090] S5. Post-processing.

[0091] The second mixed liquid is separated into solid and liquid, washed and dried to obtain spherical micro-nano copper powder.

[0092] Solid-liquid separation includes centrifugation, filtration or filter pressing; the centrifugal speed is 1000r / min-4000r / min; the number of centrifugation is 2-3 times, each time for 1-2 minutes.

[0093] The washing includes washing with deionized water for multiple times to remove the residual solvent and unreacted components on the surface.

[0094] Drying includes drying in a vacuum drying oven at 40°C-55°C for 10 min-2 h.

[0095] The particle size of the quasi-spherical micro-nano copper powder prepared by the preparation method of the quasi-spherical micro-nano copper powder is 100-400nm. The quasi-spherical micro-nano copper powder can be widely used in the preparation of conductive ink.

[0096] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0097] Example 1

[0098] This embodiment provides a method for preparing spherical micro-nano copper powder, which comprises:

[0099] (1) Weigh 5.28 g of ascorbic acid and 2.1 g of gelatin, dissolve in 50 ml of deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 65°C;

[0100] (2) Weigh 1.96 g of copper formate, 0.98 g of PVP, and 2.45 g of sodium citrate, and dissolve them in a mixture of 15 ml of deionized water and 10 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0101] (3) Weigh 0.35 g copper formate, 0.17 g PVP, and 0.44 g sodium citrate, and dissolve them in 25 ml deionized water to prepare a copper salt growth solution;

[0102] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 65°C for 2 min;

[0103] (5) After the first stage reaction stops, the first mixed solution is rapidly cooled to 40° C. within 4 min;

[0104] (6) slowly dripping the copper salt growth solution into the reaction system, and the reaction system reacts at 40° C. for 8 min;

[0105] (7) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0106] from Figure 1 It can be seen that the average particle size of the copper powder prepared in this embodiment is about 237.65nm, where D 10 =185.70nm,D 50 =246.20nm,D 90 =277.60nm, Span=0.37, the particle size distribution is uniform and spherical, the copper powders are evenly dispersed without adhesion or agglomeration.

[0107] Example 2

[0108] This embodiment provides a method for preparing spherical micro-nano copper powder, which comprises:

[0109] (1) Weigh 5.28 g of ascorbic acid and 2.1 g of gelatin, dissolve in 50 ml of deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 65°C;

[0110] (2) Weigh 1.85 g of copper formate, 0.92 g of PVP (K-90), and 1.86 g of sodium citrate, and dissolve them in a mixture of 10 ml of deionized water and 10 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0111] (3) Weigh 0.46 g of copper formate and 0.23 g of PVP (K-90), dissolve them in 25 ml of deionized water to prepare a copper salt growth solution;

[0112] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 65°C for 2 min;

[0113] (5) After the first stage reaction stops, the first mixed solution is rapidly cooled to 35° C. within 5 min;

[0114] (6) slowly dripping the copper salt growth solution into the reaction system, and the reaction system reacts at 35° C. for 8 min;

[0115] (7) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0116] from Figure 2 It can be seen that the average particle size of the copper powder prepared in this embodiment is about 169.84nm, where D 10 =135.80nm,D 50 =172.82nm,D 90 =202.69nm, Span=0.39, the particle size distribution is uniform and spherical, the copper powders are evenly dispersed without adhesion or agglomeration.

[0117] Example 3

[0118] This embodiment provides a method for preparing spherical micro-nano copper powder, which comprises:

[0119] (1) Weigh 5.28 g of ascorbic acid and 2.1 g of gelatin, dissolve in 40 ml of deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 68°C;

[0120] (2) Weigh 1.85 g of copper formate, 0.92 g of PVP (K-90), and 1.2 g of sodium citrate, and dissolve them in a mixture of 10 ml of deionized water and 10 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0121] (3) Weigh 0.46 g of copper formate and 0.23 g of PVP (K-90), dissolve them in 30 ml of deionized water to prepare a copper salt growth solution;

[0122] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 68°C for 1 min 30 s;

[0123] (5) After the first stage reaction stops, the first mixed solution is rapidly cooled to 35° C. within 5 min;

[0124] (6) slowly dripping the copper salt growth solution into the reaction system, and the reaction system reacts at 35° C. for 8 min;

[0125] (7) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0126] from Figure 3 It can be seen that the average particle size of the copper powder prepared in this embodiment is about 183.36nm, where D 10 =155.69nm,D 50 =183.91nm,D 90 =212.85nm, Span=0.31, the particle size distribution is uniform and spherical, the copper powders are evenly dispersed without adhesion or agglomeration.

[0127] Example 4

[0128] This embodiment provides a method for preparing spherical micro-nano copper powder, which comprises:

[0129] (1) Weigh 3.52 g of ascorbic acid, 0.7 g of gelatin, and 0.35 g of sodium citrate, dissolve in 50 ml of deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 85°C;

[0130] (2) Weigh 0.693 g of copper formate and 0.35 g of PVP, dissolve them in 15 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0131] (3) Weigh 0.08 g of copper formate and 0.04 g of PVP, dissolve them in 25 ml of deionized water to prepare a copper salt growth solution;

[0132] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 85°C for 3 min;

[0133] (5) After the first stage reaction stops, the first mixed solution is rapidly cooled to 45° C. within 8 min;

[0134] (6) slowly dripping the copper salt growth solution into the reaction system, and the reaction system reacts at 45° C. for 10 min;

[0135] (7) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0136] from Figure 4 It can be seen that the average particle size of the copper powder prepared in this embodiment is about 157.23 nm, where D 10 =130.01nm,D 50 =156.79nm,D 90 =187.52nm, Span=0.37, the particle size distribution is uniform and spherical, the copper powders are evenly dispersed without adhesion or agglomeration.

[0137] from Figure 5 It can be seen from the XRD diagram that there are three very sharp peaks at 43.37°, 50.49° and 74.13°, which proves that the copper powder prepared in this embodiment is pure copper, rather than copper oxide or cuprous oxide.

[0138] Example 5

[0139] This embodiment provides a method for preparing spherical micro-nano copper powder, which comprises:

[0140] (1) Weigh 2.64 g ascorbic acid, 0.7 g gelatin, and 0.35 g sodium citrate, dissolve in 50 ml deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 85°C;

[0141] (2) Weigh 0.693 g of copper formate and 0.35 g of PVP, dissolve them in 10 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0142] (3) Weigh 0.08 g of copper formate and 0.04 g of PVP, dissolve them in 25 ml of deionized water to prepare a copper salt growth solution;

[0143] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 85°C for 3 min;

[0144] (5) After the first stage reaction stops, the first mixed solution is rapidly cooled to 45° C. within 8 min;

[0145] (6) slowly dripping the copper salt growth solution into the reaction system, and the reaction system reacts at 45° C. for 10 min;

[0146] (7) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0147] from Figure 6 It can be seen that the average particle size of the copper powder prepared in this embodiment is about 256.62nm, where D 10 =215.87nm,D 50 =264.24nm,D 90 =306.57nm, Span=0.34, the particle size distribution is uniform and spherical, the copper powders are evenly dispersed without adhesion or agglomeration.

[0148] Example 6

[0149] This embodiment provides a method for preparing spherical micro-nano copper powder, which comprises:

[0150] (1) Weigh 2.64 g ascorbic acid, 0.7 g gelatin, and 0.35 g sodium citrate, dissolve in 50 ml deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 80°C;

[0151] (2) Weigh 0.693 g of copper formate and 0.35 g of PVP, dissolve them in 10 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0152] (3) Weigh 0.08 g of copper formate and 0.04 g of PVP, dissolve them in 25 ml of deionized water to prepare a copper salt growth solution;

[0153] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 80°C for 2 min;

[0154] (5) After the first stage reaction stops, the first mixed solution is rapidly cooled to 40° C. within 8 min;

[0155] (6) slowly dripping the copper salt growth solution into the reaction system, and the reaction system reacts at 40° C. for 10 min;

[0156] (7) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0157] from Figure 7 It can be seen that the average particle size of the copper powder prepared in this embodiment is about 324.95nm, where D 10 =260.97nm,D 50 =328.74nm,D 90=387.96nm, Span=0.39, the particle size distribution is uniform and spherical, the copper powders are evenly dispersed without adhesion or agglomeration.

[0158] Example 7

[0159] This embodiment provides a method for preparing spherical micro-nano copper powder, which comprises:

[0160] (1) Weigh 5.28 g of ascorbic acid, 1.4 g of gelatin, and 0.7 g of sodium citrate, dissolve in 50 ml of deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 80°C;

[0161] (2) Weigh 1.386 g of copper formate and 0.7 g of PVP, dissolve them in 15 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0162] (3) Weigh 0.15 g of copper formate and 0.08 g of PVP, dissolve them in 25 ml of deionized water to prepare a copper salt growth solution;

[0163] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 80°C for 2 min;

[0164] (5) After the first stage reaction stops, the first mixed solution is rapidly cooled to 40° C. within 8 min;

[0165] (6) slowly dripping the copper salt growth solution into the reaction system, and the reaction system reacts at 40° C. for 10 min;

[0166] (7) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0167] from Figure 8 It can be seen that the average particle size of the copper powder prepared in this embodiment is about 190.97nm, where D 10 =151.18nm,D 50 =188.71nm,D 90 =237.79nm, Span=0.46, the particle size distribution is uniform and spherical, the copper powders are evenly dispersed without adhesion or agglomeration.

[0168] from Fig. 9 and Fig.10 It can be seen that the copper powders are evenly dispersed without any adhesion or agglomeration.

[0169] Example 8

[0170] This embodiment provides a method for preparing spherical micro-nano copper powder, which comprises:

[0171] (1) Weigh 10.56 g ascorbic acid, 2.1 g gelatin, and 1.05 g sodium citrate, dissolve in 50 ml deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 85°C;

[0172] (2) Weigh 2.08 g of copper formate and 1.04 g of PVP, dissolve them in 15 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0173] (3) Weigh 0.23 g of copper formate and 0.12 g of PVP, dissolve them in 25 ml of deionized water to prepare a copper salt growth solution;

[0174] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 85°C for 3 min;

[0175] (5) After the first stage reaction stops, the first mixed solution is rapidly cooled to 45° C. within 10 min;

[0176] (6) slowly dripping the copper salt growth solution into the reaction system, and the reaction system reacts at 45° C. for 10 min;

[0177] (7) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0178] from Fig.11 It can be seen that the average particle size of the copper powder prepared in this embodiment is about 345.41nm, where D 10 =252.37nm,D 50 =351.44nm,D 90 =430.94nm, Span=0.51, the particle size distribution is uniform and spherical, the copper powders are evenly dispersed without adhesion or agglomeration.

[0179] Example 9

[0180] This embodiment provides a method for preparing spherical micro-nano copper powder, which comprises:

[0181] (1) Weigh 5.28 g of ascorbic acid and 2.1 g of gelatin, dissolve in 50 ml of deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 70°C;

[0182] (2) Weigh 1.85 g of copper formate, 0.92 g of PVP, and 2.32 g of sodium citrate, and dissolve them in a mixture of 10 ml of deionized water and 15 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0183] (3) Weigh 0.46 g copper formate, 0.23 g PVP, and 0.58 g sodium citrate, and dissolve them in 25 ml deionized water to prepare a copper salt growth solution;

[0184] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 70°C for 2 min;

[0185] (5) After the first stage reaction stops, the first mixed solution is rapidly cooled to 40° C. within 8 min;

[0186] (6) slowly dripping the copper salt growth solution into the reaction system, and the reaction system reacts at 40° C. for 8 min;

[0187] (7) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0188] from Fig.12 It can be seen that the average particle size of the copper powder prepared in this embodiment is about 166.66nm, where D 10 =136.19nm,D 50 =166.70nm,D 90 =203.32nm, Span = 0.40, the particle size distribution is uniform and spherical, the copper powders are evenly dispersed without adhesion or agglomeration.

[0189] Example 10

[0190] This embodiment provides a method for preparing spherical micro-nano copper powder, which comprises:

[0191] (1) Weigh 5.28 g of ascorbic acid and 2.1 g of gelatin, dissolve in 50 ml of deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 65°C;

[0192] (2) Weigh 1.85 g of copper formate, 0.92 g of PVP, and 2.32 g of sodium citrate, and dissolve them in a mixture of 15 ml of deionized water and 10 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0193] (3) Weigh 0.46 g copper formate, 0.23 g PVP, and 0.58 g sodium citrate, and dissolve them in 25 ml deionized water to prepare a copper salt growth solution;

[0194] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 65°C for 2 min;

[0195] (5) After the first stage reaction stops, the first mixed solution is rapidly cooled to 40° C. within 4 min;

[0196] (6) slowly dripping the copper salt growth solution into the reaction system, and the reaction system reacts at 40° C. for 8 min;

[0197] (7) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0198] from Fig.13 It can be seen that the average particle size of the copper powder prepared in this embodiment is about 132.07nm, where D 10 =108.33nm,D 50 =130.09nm,D 90 =158.01nm, Span=0.38, the particle size distribution is uniform and spherical, the copper powders are evenly dispersed without adhesion or agglomeration.

[0199] Embodiment 11

[0200] This embodiment provides a method for preparing spherical micro-nano copper powder, which comprises:

[0201] (1) Weigh 5.28 g of ascorbic acid and 2.1 g of gelatin, dissolve in 50 ml of deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 65°C;

[0202] (2) Weigh 1.85 g of copper formate, 0.92 g of PVP, and 2.32 g of sodium citrate, and dissolve them in a mixture of 20 ml of deionized water and 5 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0203] (3) Weigh 0.46 g copper formate, 0.23 g PVP, and 0.58 g sodium citrate, and dissolve them in 25 ml deionized water to prepare a copper salt growth solution;

[0204] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 60°C for 2 min;

[0205] (5) After the first stage reaction stops, the first mixed solution is rapidly cooled to 40° C. within 4 min;

[0206] (6) slowly dripping the copper salt growth solution into the reaction system, and the reaction system reacts at 40° C. for 8 min;

[0207] (7) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0208] from Fig.14 It can be seen that the average particle size of the copper powder prepared in this embodiment is about 399.49 nm, where D10 =330.67nm,D 50 =406.37nm,D 90 =468.20nm, Span=0.34, the particle size distribution is uniform and spherical, the copper powders are evenly dispersed without adhesion or agglomeration.

[0209] Comparative Example 1

[0210] This comparative example provides a method for preparing copper powder, which comprises the following steps:

[0211] (1) Weigh 1.76 g of ascorbic acid and 1.15 g of gelatin, dissolve in 50 ml of deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 60°C;

[0212] (2) Weigh 0.625 g of copper sulfate pentahydrate and 0.58 g of PVP, dissolve them in 25 ml of deionized water to prepare a copper salt nucleation solution;

[0213] (3) Weigh 0.625 g of copper sulfate pentahydrate and 0.58 g of PVP, dissolve them in 25 ml of deionized water to prepare a copper salt growth solution;

[0214] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 60°C for 5 min;

[0215] (5) After the first stage reaction stops, the copper salt growth solution is slowly dripped into the reaction system, and the reaction system is reacted at 60°C for 15 minutes;

[0216] (6) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0217] from Fig.15 It can be seen that the average particle size of the copper powder prepared in this comparative example is about 3890.20nm, where D 10 =2695.84nm,D 50 =3869.12nm,D 90 =4974.24nm, Span=0.59, the particle size distribution is relatively uniform, irregular in shape, poor in sphericity, and the copper powders are evenly dispersed without adhesion or agglomeration.

[0218] Comparative Example 2

[0219] This comparative example provides a method for preparing copper powder, which comprises the following steps:

[0220] (1) Weigh 1.76 g of ascorbic acid and dissolve it in 50 ml of deionized water to prepare a reducing base solution. Transfer the solution to a heating mantle and heat it to 60°C.

[0221] (2) Weigh 0.77 g of copper formate and 1.15 g of PVP, dissolve them in 50 ml of deionized water to prepare a copper salt precursor solution;

[0222] (3) Slowly drip the reducing base solution into the copper salt precursor solution and react at 60°C for 20 minutes;

[0223] (4) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum drying oven at 45° C. for 1 h to remove the copper powder.

[0224] from Fig.16 It can be seen that the average particle size of the copper powder prepared in this comparative example is about 2891.40nm, where D 10 =2206.34nm,D 50 =2896.26nm,D 90 =3486.15nm, Span=0.44, the particle size is relatively large, the particle size distribution is relatively uniform, and it is spherical, but there is obvious adhesion or agglomeration between the copper powders.

[0225] Comparative Example 3

[0226] This comparative example provides a method for preparing copper powder, which comprises the following steps:

[0227] (1) Weigh 3.52 g of ascorbic acid and 2.3 g of PVP, dissolve in 50 ml of deionized water to prepare a reducing base solution, transfer to a heating mantle, and heat to 70°C;

[0228] (2) Weigh 0.58 g of copper formate, 1.15 g of PVP, and 2.5 g of sodium citrate, and dissolve them in 25 ml of deionized water to prepare a copper salt nucleation solution;

[0229] (3) Weigh 0.19 g copper formate, 1.15 g PVP, and 2.5 g sodium citrate, and dissolve them in 25 ml deionized water to prepare a copper salt growth solution;

[0230] (4) Pour the copper salt nucleation solution into the reducing base solution instantly and react at 70°C for 5 min;

[0231] (5) After the first stage reaction stops, the copper salt growth solution is slowly dripped into the reaction system, and the reaction system is reacted at 70°C for 15 minutes;

[0232] (6) Stop the reaction, centrifuge the reactants at 3000 r / min for 1 min each time, wash, filter, and dry in a vacuum oven at 45° C. for 1 h to remove the copper powder.

[0233] from Fig.17 It can be seen that the average particle size of the copper powder prepared in this comparative example is about 842.81nm, where D 10 =723.69nm,D 50 =847.30nm,D 90 =946.90nm, Span = 0.26, the particle size distribution is relatively uniform and spherical, but there is obvious adhesion or agglomeration between the copper powders.

[0234] Comparative Example 4

[0235] This comparative example is basically the same as Example 1, except that the rapid freezing of step (5) of Example 1 is omitted in this comparative example. The copper salt growth solution is directly dripped into the reaction system slowly, and the reaction system is reacted at 65° C. for 8 minutes.

[0236] from Fig.18 It can be seen that omitting the rapid freezing step will lead to a rapid entry into the growth stage after nucleation, and the morphology is difficult to control, resulting in the average particle size of the copper powder finally prepared being about 691.77nm, where D 10 =522.90nm,D 50 =713.33nm,D 90 =860.92nm, Span=0.473, the particle size distribution is relatively uniform, but the particle size is significantly larger than that in Example 1, and the morphology of the copper powder is irregular, and there is obvious adhesion or agglomeration between the copper powders.

[0237] Comparative Example 5

[0238] This comparative example is basically the same as Example 1, except that in step (5) of this comparative example, the cooling is carried out directly at room temperature and then slowly cooled to 40° C. for 20 min.

[0239] from Fig.19 It can be seen that the comparative example is cooled at room temperature, the cooling time is long, the morphology is difficult to control, and the average particle size of the prepared copper powder is about 1013.91nm, where D 10 =803.14nm,D 50 =1011.54nm,D 90 =1171.95nm, Span=0.365, the particle size distribution is relatively uniform, but the particle size is significantly larger than that in Example 1, and the morphology of the copper powder is irregular.

[0240] Comparative Example 6

[0241] This comparative example is basically the same as Example 1, except that steps (2) and (3) in this comparative example are different from those in Example 1, and the ratio of the concentration of copper formate in the copper salt nucleation solution and the copper salt growth solution in this comparative example is 6:4. Specifically:

[0242] (2) Weigh 1.386 g of copper formate, 0.98 g of PVP, and 2.45 g of sodium citrate, and dissolve them in a mixture of 15 ml of deionized water and 10 ml of ethylene glycol to prepare a copper salt nucleation solution;

[0243] (3) Weigh 0.924 g of copper formate, 0.17 g of PVP, and 0.44 g of sodium citrate, and dissolve them in 25 ml of deionized water to prepare a copper salt growth solution.

[0244] from Fig. 20 It can be seen that when the concentration ratio of copper formate in the copper salt nucleation solution and the copper salt growth solution is reduced, the nucleation speed will be slow, but the growth speed will be fast, which will greatly increase the size of the obtained copper particles and have an adverse effect on the preparation effect. The average particle size of the copper powder prepared in this comparative example is about 690.89nm, where D 10 =509.16nm, D 50 =656.37nm, D 90 =769.61nm, Span=0.397, the particle size distribution uniformity is poor, the particle shape is spherical, and there is obvious adhesion or agglomeration between the copper powders.

[0245] Comparative Example 7

[0246] This comparative example is basically the same as Example 1, except that the first-stage reaction time of step (4) in this comparative example is 5 minutes.

[0247] from Fig.21 It can be seen that the extension of the reaction time in the first stage will lead to excessive nucleation and rapid increase in the volume of the copper powder. Therefore, the average particle size of the copper powder prepared in this comparative example is about 660.75nm, where D 10 =550.33nm,D 50 =673.38nm,D 90 =804.23nm, Span=0.377, the particle size distribution is relatively uniform, spherical, and the copper powders are obviously bonded or agglomerated. It can be seen that the particle size of comparative example 7 is twice larger than that of example 1 (237.65nm), and there are bonding and agglomeration phenomena, which fully proves that the nucleation time should not be too long.

[0248] Comparative Example 8

[0249] This comparative example is substantially the same as Example 1, except that the copper formate in Example 1 is replaced by copper sulfate pentahydrate in this comparative example.

[0250] from Fig. 22It can be seen that in Comparative Example 8, copper formate is replaced by copper sulfate pentahydrate, and the average particle size of the copper powder prepared in this comparative example is about 1349.46 nm, wherein D 10 =1158.30nm,D 50 =1374.21nm,D 90 =1592.23nm, Span=0.316, the particle size distribution uniformity is poor, irregular, and the particle size is significantly larger than that of Example 1, and the copper powders are evenly dispersed without adhesion or agglomeration. Therefore, it can be seen that the selection of copper source has a significant effect on the particle size of the final copper powder.

[0251] Comparative Example 9

[0252] This comparative example is substantially the same as Example 1, except that the gelatin in Example 1 is replaced by PVP in this comparative example.

[0253] from Fig.23 It can be seen that replacing gelatin with a conventional dispersant in this comparative example will result in poor dispersion effect. The average particle size of the copper powder prepared in this comparative example is about 1182.73 nm, where D 10 =755.8nm,D 50 =1251.09nm,D 90 =1484.64nm, Span=0.582, the particle size distribution is relatively uniform, spherical, and the particle size is significantly larger than that of Example 1, and there is obvious adhesion or agglomeration between the copper powders.

[0254] The experimental results of the above embodiments and comparative examples are summarized as follows:

[0255]

[0256]

[0257] From the statistics in the above table, it can be seen that the copper powder prepared by the preparation method of the spherical micro-nano copper powder provided in the embodiment of the present invention has a small particle size, an average particle size of less than 400nm, and a uniform particle size distribution without obvious agglomeration. In comparative examples 1-9, the particle size is significantly increased, and the particle size of comparative example 7 with the smallest particle size also reaches 660.75nm, which is significantly higher than that of embodiments 1-11 of the present invention, and the maximum particle size of the comparative example reaches 3890.20nm, which is extremely significantly increased compared with embodiments 1-11 of the present invention, and many of the comparative examples have agglomeration phenomena, which fully proves that the embodiment of the present invention is significantly better than the comparative example.

[0258] In summary, the preparation method of quasi-spherical micro-nano copper powder provided by the present invention is to prepare quasi-spherical micro-nano copper powder by two-stage reaction and rapid cooling. After the first stage reaction is completed, rapid cooling can effectively separate the nucleation and growth processes involved in the formation of copper particles, thereby achieving the effect of limiting particle size and agglomeration and maintaining excellent particle size distribution. At the same time, the temperature of the second stage reaction is lower than the temperature of the first stage reaction, and the reaction time is greater than the time of the first stage reaction, so that the reaction system reacts for a short time under high temperature conditions in the first stage reaction, and reacts for a longer time at a lower temperature in the second stage reaction, which can "explosively" form a large number of copper nuclei in a short time. The copper formate content of the copper salt nucleation liquid and the copper salt growth liquid is quite different, which can achieve the purpose of "large nucleation + slow growth". The copper powder prepared by the preparation method of quasi-spherical micro-nano copper powder provided by the present invention has a small particle size, a uniform particle size distribution and no obvious agglomeration phenomenon. It can be widely used in the preparation of conductive inks.

[0259] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing spherical micro-nano copper powder, characterized in that: It includes: The reducing base liquid and the copper salt nucleation liquid are mixed, and the first stage reaction is carried out at 50°C-90°C for 0.5min-4min to obtain a first mixed liquid; wherein the reducing base liquid comprises 0.02g / ml-0.50g / ml of ascorbic acid and 0.01g / ml-0.10g / ml of gelatin, and the copper salt nucleation liquid comprises 0.02g / ml-0.25g / ml of copper formate; Rapidly cool the first mixed solution to 20°C-45°C within 3-15 minutes; Injecting the copper salt growth solution into the cooled first mixed solution to carry out a second stage reaction, the reaction time is 6 min-20 min; obtaining a second mixed solution; wherein the copper salt growth solution comprises 0.003 g / ml-0.018 g / ml of copper formate; The second mixed liquid is separated into solid and liquid, washed and dried to obtain spherical micro-nano copper powder.

2. The method for preparing spherical micro-nano copper powder according to claim 1, characterized in that: Before the reducing base liquid and the copper salt nucleation liquid are mixed, the copper salt nucleation liquid and the reducing base liquid are heated and kept warm respectively; Preferably, the holding temperature of the copper salt nucleation solution is 43°C-75°C; Preferably, the insulation temperature of the reducing base solution is 50°C-90°C; Preferably, the mixing method of the reducing base liquid and the copper salt nucleation liquid comprises adding the copper salt nucleation liquid into the reducing base liquid.

3. The method for preparing spherical micro-nano copper powder according to claim 1, characterized in that: The copper formate in the copper salt nucleation solution accounts for 80%-90% of the total mass of the copper formate in the copper salt nucleation solution and the copper salt growth solution.

4. The method for preparing spherical micro-nano copper powder according to claim 1, characterized in that: The copper salt nucleation solution also includes PVP 0.02g / ml-0.20g / ml, and the copper salt growth solution also includes PVP 0.001g / ml-0.20g / ml; Preferably, the copper salt nucleation solution further includes 0.02 g / ml-0.30 g / ml of sodium citrate, and the copper salt growth solution further includes 0.01 g / ml-0.06 g / ml of sodium citrate.

5. The method for preparing spherical micro-nano copper powder according to any one of claims 1 to 4, characterized in that: The solvents of the reducing base liquid and the copper salt growth liquid are both water, and the solvent of the copper salt nucleation liquid is ethylene glycol or a mixture of ethylene glycol and water in a volume ratio of 1:(1-6).

6. The method for preparing spherical micro-nano copper powder according to any one of claims 1 to 4, characterized in that: The copper salt growth liquid is injected into the first mixed liquid through an injection pump, the injection speed is 250ml / h-1200ml / h, and the system temperature is maintained at 20°C-45°C after injection.

7. The method for preparing spherical micro-nano copper powder according to any one of claims 1 to 4, characterized in that: The first stage reaction and the second stage reaction are both carried out under stirring, and the stirring speed is 300r / min-1200r / min.

8. The method for preparing spherical micro-nano copper powder according to any one of claims 1 to 4, characterized in that: The solid-liquid separation includes centrifugation, filtration or filter pressing; Preferably, the centrifugal speed is 1000r / min-4000r / min; Preferably, the centrifugation is performed 2-3 times, each time for 1 min-2 min; Preferably, the drying comprises drying in a vacuum drying oven at 40°C-55°C for 10 min-2 h.

9. A spherical micro-nano copper powder, characterized in that: It is prepared by the method for preparing spherical micro-nano copper powder as described in any one of claims 1 to 8; Preferably, the particle size of the quasi-spherical micro-nano copper powder is 100nm-400nm.

10. Use of the spherical micro-nano copper powder according to claim 9 in preparing conductive ink.

Citation Information

Cited By

  • Preparation method of nano copper powder

    CN120644677A

  • A method for preparing nano-copper powder

    CN123079978A