Preparation method of size-adjustable silver nanosheet

By using Gemini surfactant and silver nitrate etching technology, silver nanosheets are ensured to grow along the crystal surface of {111}, solving the problem of regulating the size and morphology of silver nanosheets in the existing technology, achieving preparation of different sizes and high yields, and improving the Its value in a variety of applications.

CN118905236AActive Publication Date: 2024-11-08QUANZHOU NORMAL UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410994400.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The prior art is difficult to effectively regulate the size and morphology of silver nanosheets, which limits its application value in the fields of sterilization, solar cells, organic light emitting diodes, medical imaging, etc.

Method used

Gemini surfactant is used as an inducer and coating agent to ensure that silver nanosheets grow along the {111} crystal plane by controlling silver nitrate etching and pH adjustment, and silver nanosheets of different sizes are prepared.

Benefits of technology

The size of silver nanosheets has been successfully controlled on a large scale, improving yield and morphology control, and is suitable for a variety of high-performance applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905236A_ABST
    Figure CN118905236A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a size-adjustable silver nanosheet, which is characterized in that the morphology of a product is controlled by using a seed crystal etched by silver nitrate, specifically, the seed crystal is oxidized by using silver nitrate, so that more {111} crystal faces are exposed on the surface of the seed crystal, and meanwhile, a proper gemini surfactant is used as a coating agent, so that the size-adjustable silver nanosheet is prepared. And tightly coating the {111} crystal face, so that the seed crystal grows along the direction parallel to the {111} crystal face, thereby obtaining the silver nanosheet of which the size is adjustable in a large range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano silver materials, and in particular to a method for preparing size-adjustable silver nano sheets. Background Art

[0002] Silver nanosheets, due to their sharp vertices, have unique optical and electrical properties. The orientation ratio is usually used as an indicator to measure the anisotropy of silver nanosheets. The orientation ratio of a nanosheet refers to the value of its side length divided by its thickness. In particular, when the nanosheet is large enough and thin enough, that is, when it has a large enough orientation ratio, it not only exhibits dipole plasma resonance, but also quadruple plasma resonance, with multiple absorption peaks in the ultraviolet visible region. Structure determines performance. Silver nanosheets have a wide range of applications in sterilization, solar cells, organic light-emitting diodes, medical imaging, optical limiters, conductive inks, antibacterial, catalysis and other fields.

[0003] In order to synthesize silver nanowires, the crystal structure of silver nanosheets must first be determined. Characterization results show that the upper and lower main crystal planes of silver nanosheets are {111} crystal planes. Therefore, the key to synthesizing silver nanosheets is to control the crystal growth direction so that it grows in a direction parallel to the {111} crystal plane.

[0004] Different reagents have a significant effect on regulating the size and morphology of silver nanomaterials. The type of surfactant directly affects the final morphology of the nanostructure. Surfactant molecules tend to aggregate in aqueous solution with polar groups facing the aqueous phase and non-polar groups away from the aqueous phase. The aggregation behavior of surfactants in solution is affected by their own molecular structure, and gemini surfactants have two hydrophobic tail chains, so they are more hydrophobic than single-chain surfactants. When the distance between the connecting chains is short, the distance between the head groups in the molecule is greatly reduced. These factors enable gemini surfactants to form a tighter adsorption layer at the gas-liquid interface, making them more efficient and effective in reducing the surface tension of water. And due to the high variability of the molecular structure of gemini surfactants, they can form a rich variety of aggregate morphologies in aqueous solution, such as spherical micelles, ellipsoidal micelles, rod-shaped micelles, disc-shaped micelles, linear micelles, vesicles, lamellar phases, liquid crystals, sponge phases, etc. Their different aggregate morphologies may have a certain effect on the shape and size of silver nanostructures. Therefore, gemini surfactants have excellent performance, significantly superior to single-chain surfactants in most properties, and can be molecularly designed according to needs to achieve the purpose of regulating the structure of nanomaterials. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing size-adjustable silver nanosheets. The preparation method is simple to operate, and the whole process is carried out under normal pressure. By using a suitable gemini surfactant, silver nanosheets with adjustable sizes in a wide range can be prepared.

[0006] In order to achieve the above object, the solution of the present invention is:

[0007] A method for preparing size-adjustable silver nanosheets comprises the following steps:

[0008] Step 1, preparation of seed crystals:

[0009] First, 1 mL of 5% to 50% (w / v) AgNO3 aqueous solution was added to 9 mL of 0.5% to 10% (w / v) gemini surfactant aqueous solution under stirring, and then 2 mL of 5% to 50% (w / v) freshly prepared NaBH4 aqueous solution was added under vigorous stirring, and the mixture was allowed to stand for 2 to 4 hours to obtain seed crystal A;

[0010] Step 2: Etching of seed crystal:

[0011] Then, 0.2-2 mL of seed crystal A was added to 9 mL of 0.5%-10% (w / v) aqueous solution of gemini surfactant, followed by 1 mL of 10%-50% (w / v) AgNO3 aqueous solution, and the temperature was raised to 40-70°C and kept for 0.5-4 h to complete the etching of the seed crystal. The obtained product was recorded as seed crystal B;

[0012] Step 3: One-step growth of seed crystal:

[0013] After the obtained seed crystal B is cooled to room temperature, concentrated ammonia is added to adjust the pH value to 8-11, and then 10 mL of 1%-10% (w / v) ascorbic acid aqueous solution is added and stirred evenly, and finally the reaction solution is allowed to stand at 25° C. for 1-14 hours to allow the reaction to proceed fully, thereby obtaining a dispersion of silver nanosheets, wherein the average particle size of the silver nanosheets is regulated within the range of 100-2000 nm;

[0014] In step 1 and step 2, the gemini surfactant is a quaternary ammonium salt surfactant, and its molecular structure is shown in Formula I:

[0015]

[0016] Among them, when s=4, the gemini surfactant is recorded as 16-4-16, when s=6, the gemini surfactant is recorded as 16-6-16, and when s=10, the gemini surfactant is recorded as 16-10-16.

[0017] Furthermore, the method further includes step 4, a two-step growth of the seed crystal:

[0018] 0.2-2 mL of the dispersion of silver nanosheets prepared in step 3 is added to 9 mL of an aqueous solution of 0.5%-10% (w / v) gemini surfactant, followed by adding 1 mL of an aqueous solution of 5%-50% (w / v) AgNO3, and then adding concentrated ammonia to adjust the pH value to 8-11, followed by adding 10 mL of an aqueous solution of 2%-10% (w / v) ascorbic acid and stirring evenly, and finally the reaction solution is allowed to stand at 25°C for 1-14 h to allow the reaction to proceed fully, to obtain a dispersion of silver nanosheets, the average particle size of which is regulated within the range of 2000-5000 nm.

[0019] In step 4, the gemini surfactant is a quaternary ammonium salt surfactant, and its molecular structure is shown in Formula I:

[0020]

[0021] Among them, when s=4, the gemini surfactant is recorded as 16-4-16, when s=6, the gemini surfactant is recorded as 16-6-16, and when s=10, the gemini surfactant is recorded as 16-10-16.

[0022] In step 4, the dispersion of the silver nanosheets obtained by the reaction is centrifuged, washed, and finally dispersed in water for storage; or dried at 80-100° C. for 4-24 hours to obtain a powdered solid.

[0023] In step 3, the concentration of the concentrated ammonia water is 25% to 28% (w / v).

[0024] In step 3, the dispersion of the silver nanosheets obtained by the reaction is centrifuged, washed, and finally dispersed in water for storage; or dried at 80-100° C. for 4-24 hours to obtain a powdered solid.

[0025] After adopting the above technical solution, the method for preparing size-adjustable silver nanosheets of the present invention has the following advantages:

[0026] First, a quaternary ammonium surfactant is used as an inducer to synthesize silver nanosheets of desired shape and size. The molecular structure of the quaternary ammonium surfactant is shown in Formula I. The intermediate connecting chain can be adjusted as needed, which is also one of the key factors for the invention to form high-yield silver nanosheets. Since the gemini surfactant can form abundant aggregate structures in water, its different aggregate structures may have a certain influence on the shape and size of the silver nanostructure. Therefore, the invention successfully synthesizes silver nanosheets of different sizes by changing the length of the intermediate connecting chain. However, the use of traditional single-chain surfactants such as CTAB can only form nanoparticles or low-yield nanosheets.

[0027] The second is the innovation of the preparation method. It is a very challenging problem to customize the size of the silver nanosheet according to the demand. The present invention achieves this goal by the following method: Since the corrosion of the crystal surface of the silver nanosheet side by silver nitrate is much faster than the corrosion of the crystal surface at both ends of the nanorod, and since the crystal surface of the former is a non-{111} crystal surface, while the latter is a {111} crystal surface, that is, the corrosion of the {111} crystal surface by silver nitrate is slower. Inspired by this, the present invention attempts to control the morphology of the product by using seeds etched by silver nitrate. Specifically, the seeds are oxidized by silver nitrate so that more {111} crystal surfaces are exposed on the surface of the seeds. At the same time, an appropriate quaternary ammonium salt gemini surfactant is used as a coating agent and tightly coated on the {111} crystal surface, so that it grows in a direction parallel to the {111} crystal surface, and by adjusting the length of the intermediate connecting chain of the gemini surfactant, the amount of seed added, and the pH value, etc., silver nanosheets with a large size controllable range are obtained. The preparation method is simple to operate, the whole process is carried out under normal pressure, and the operability is strong. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a SEM image of the silver nanosheets prepared in Example 1;

[0029] Figure 2 This is a SEM image of the silver nanosheets prepared in Example 2;

[0030] Figure 3 This is a SEM image of the silver nanosheets prepared in Example 3;

[0031] Figure 4 This is a SEM image of the silver nanosheets prepared in Example 4;

[0032] Figure 5 This is a SEM image of the silver nanosheets prepared in Example 5;

[0033] Figure 6 This is a SEM image of the silver nanosheets prepared in Example 6;

[0034] Figure 7 This is a SEM image of the silver nanosheets prepared in Example 7;

[0035] Figure 8 This is a SEM image of the silver nanosheets prepared in Example 8;

[0036] Fig. 9 This is the SEM image of the silver nanosheets prepared in Example 9. DETAILED DESCRIPTION

[0037] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.

[0038] Example 1

[0039] A method for preparing size-adjustable silver nanosheets comprises the following steps:

[0040] Step 1, preparation of seed crystals:

[0041] First, 1 mL of 10% (w / v) AgNO3 aqueous solution was added to 9 mL of 2% (w / v) Gemini surfactant 16-4-16 aqueous solution under stirring, and then 2 mL of 10% (w / v) freshly prepared NaBH4 aqueous solution was added under vigorous stirring, and the mixture was allowed to stand for 2 h to obtain seed crystal A;

[0042] Step 2: Etching of seed crystal:

[0043] Then, 0.2 mL of seed A was added to 9 mL of 2% (w / v) aqueous solution of gemini surfactant 16-4-16, followed by 1 mL of 10% to 50% (w / v) AgNO3 aqueous solution, and the temperature was raised to 40°C and kept for 0.5 h to complete the etching of the seed. The obtained product was recorded as seed B.

[0044] Step 3: One-step growth of seed crystal:

[0045] After the obtained seed crystal B was cooled to room temperature, 25% (w / v) concentrated ammonia water was added to adjust the pH value to 8, followed by adding 10 mL of 1% (w / v) ascorbic acid aqueous solution and stirring evenly, and then the reaction solution was allowed to stand at 25° C. for 1 h to allow the reaction to proceed fully to obtain a dispersion of silver nanosheets. The obtained dispersion of silver nanosheets was centrifuged at a speed of 200 r / min, washed with deionized water, and finally dispersed in water for storage; the SEM image of the silver nanosheets is shown in FIG. Figure 1 As shown, the average particle size is between 800 and 1000 nm.

[0046] In step 1 and step 2, the molecular structure of the gemini surfactant 16-4-16 is shown below, where s=4.

[0047]

[0048] Example 2

[0049] A method for preparing size-adjustable silver nanosheets comprises the following steps:

[0050] Step 1, preparation of seed crystals:

[0051] First, 1 mL of 10% (w / v) AgNO3 aqueous solution was added to 9 mL of 0.5% (w / v) Gemini surfactant 16-6-16 aqueous solution under stirring, and then 2 mL of 10% (w / v) freshly prepared NaBH4 aqueous solution was added under vigorous stirring, and the mixture was allowed to stand for 4 hours to obtain seed crystal A;

[0052] Step 2: Etching of seed crystal:

[0053] Then, 0.5 mL of seed A was added to 9 mL of 0.5% (w / v) aqueous solution of gemini surfactant 16-6-16, followed by 1 mL of 10% (w / v) AgNO3 aqueous solution, and the temperature was raised to 60°C and kept for 4 h to complete the etching of the seed. The obtained product was recorded as seed B.

[0054] Step 3: One-step growth of seed crystal:

[0055] After the obtained seed crystal B was cooled to room temperature, 25% (w / v) concentrated ammonia water was added to adjust the pH value to 11, and then 10 mL of 1% (w / v) ascorbic acid aqueous solution was added and stirred evenly, and then the reaction solution was allowed to stand at 25° C. for 4 h to allow the reaction to proceed fully to obtain a dispersion of silver nanosheets. The obtained dispersion of silver nanosheets was centrifuged at a speed of 200 r / min, washed with deionized water, and finally dispersed in water for storage; the SEM image of the silver nanosheets is shown in FIG. Figure 2 As shown, the average particle size is between 500 and 1000 nm.

[0056] In step 1 and step 2, the molecular structure of the gemini surfactant 16-6-16 is shown below, where s=6.

[0057]

[0058] Example 3

[0059] A method for preparing size-adjustable silver nanosheets comprises the following steps:

[0060] Step 1, preparation of seed crystals:

[0061] First, 1 mL of 10% (w / v) AgNO3 aqueous solution was added to 9 mL of 2% (w / v) Gemini surfactant 16-4-16 aqueous solution under stirring, and then 2 mL of 10% (w / v) freshly prepared NaBH4 aqueous solution was added under vigorous stirring, and the mixture was allowed to stand for 2 h to obtain seed crystal A;

[0062] Step 2: Etching of seed crystal:

[0063] Then, 0.2 mL of seed A was added to 9 mL of 4% (w / v) aqueous solution of gemini surfactant 16-4-16, followed by 1 mL of 10% (w / v) AgNO3 aqueous solution, and the temperature was raised to 50°C and kept for 0.5 h to complete the etching of the seed. The obtained product was recorded as seed B.

[0064] Step 3: One-step growth of seed crystal:

[0065] After the obtained seed crystal B was cooled to room temperature, 25% (w / v) concentrated ammonia water was added to adjust the pH value to 9, followed by adding 10 mL of 1% (w / v) ascorbic acid aqueous solution and stirring evenly, and then the reaction solution was allowed to stand at 25° C. for 14 h to allow the reaction to proceed fully to obtain a dispersion of silver nanosheets. The obtained dispersion of silver nanosheets was centrifuged at a speed of 200 r / min, washed with deionized water, and finally dispersed in water for storage; the SEM image of the silver nanosheets is shown in FIG. Figure 3 As shown, the average particle size is between 1000 and 1800 nm.

[0066] In step 1 and step 2, the molecular structure of the gemini surfactant 16-4-16 is shown below, where s=4.

[0067]

[0068] Example 4

[0069] A method for preparing size-adjustable silver nanosheets comprises the following steps:

[0070] Step 1, preparation of seed crystals:

[0071] First, 1 mL of 10% (w / v) AgNO3 aqueous solution was added to 9 mL of 3% (w / v) Gemini surfactant 16-10-16 aqueous solution under stirring, and then 2 mL of 10% (w / v) freshly prepared NaBH4 aqueous solution was added under vigorous stirring, and the mixture was allowed to stand for 2 h to obtain seed crystal A;

[0072] Step 2: Etching of seed crystal:

[0073] Then, 0.6 mL of seed A was added to 9 mL of 2% (w / v) aqueous solution of gemini surfactant 16-10-16, followed by 1 mL of 10% (w / v) AgNO3 aqueous solution, and the temperature was raised to 60°C and kept for 2 h to complete the etching of the seed. The obtained product was recorded as seed B.

[0074] Step 3: One-step growth of seed crystal:

[0075] After the obtained seed crystal B was cooled to room temperature, 25% (w / v) concentrated ammonia water was added to adjust the pH value to 8, and then 10 mL of 2% (w / v) ascorbic acid aqueous solution was added and stirred evenly, and then the reaction solution was allowed to stand at 25° C. for 14 h to allow the reaction to proceed fully to obtain a dispersion of silver nanosheets. The dispersion of silver nanosheets was centrifuged at a speed of 300 r / min, washed with deionized water, and finally dispersed in water for storage; the SEM image of the silver nanosheets is shown in FIG. Figure 4 As shown, the average particle size is between 400 and 1000 nm.

[0076] In step 1 and step 2, the molecular structure of the Gemini surfactant 16-10-16 is as shown below, wherein s=10.

[0077]

[0078] Example 5

[0079] A method for preparing size-adjustable silver nanosheets comprises the following steps:

[0080] Step 1, preparation of seed crystals:

[0081] First, 1 mL of 10% (w / v) AgNO3 aqueous solution was added to 9 mL of 10% (w / v) Gemini surfactant 16-4-16 aqueous solution under stirring, and then 2 mL of 10% (w / v) freshly prepared NaBH4 aqueous solution was added under vigorous stirring, and the mixture was allowed to stand for 2 h to obtain seed crystal A;

[0082] Step 2: Etching of seed crystal:

[0083] Then, 1 mL of seed A was added to 9 mL of 10% (w / v) aqueous solution of gemini surfactant 16-4-16, followed by 1 mL of 10% (w / v) aqueous AgNO3 solution, and the temperature was raised to 40°C and kept for 4 h to complete the etching of the seed. The obtained product was recorded as seed B.

[0084] Step 3: One-step growth of seed crystal:

[0085] After the obtained seed crystal B was cooled to room temperature, 25% (w / v) concentrated ammonia water was added to adjust the pH value to 10, followed by adding 10 mL of 2% (w / v) ascorbic acid aqueous solution and stirring evenly, and finally the reaction solution was allowed to stand at 25° C. for 14 h to allow the reaction to proceed fully to obtain a dispersion of silver nanosheets. The obtained dispersion of silver nanosheets was centrifuged at a speed of 200 r / min, washed with deionized water, and finally dried at 80° C. for 12 h to obtain a powdered solid; the SEM image of the silver nanosheets is shown in FIG. Figure 5 As shown, the average particle size is between 200 and 500 nm.

[0086] In step 1 and step 2, the molecular structure of the gemini surfactant 16-4-16 is as shown below, wherein s=4.

[0087]

[0088] Example 6

[0089] A method for preparing size-adjustable silver nanosheets comprises the following steps:

[0090] Step 1, preparation of seed crystals:

[0091] First, 1 mL of 10% (w / v) AgNO3 aqueous solution was added to 9 mL of 6% (w / v) Gemini surfactant 16-4-16 aqueous solution under stirring, and then 2 mL of 10% (w / v) freshly prepared NaBH4 aqueous solution was added under vigorous stirring, and the mixture was allowed to stand for 2 h to obtain seed crystal A;

[0092] Step 2: Etching of seed crystal:

[0093] Then, 2 mL of seed A was added to 9 mL of 6% (w / v) aqueous solution of gemini surfactant 16-4-16, followed by 1 mL of 10% (w / v) AgNO3 aqueous solution, and the temperature was raised to 70°C and kept for 0.5 h to complete the etching of the seed. The obtained product was recorded as seed B.

[0094] Step 3: One-step growth of seed crystal:

[0095] After the obtained seed crystal B was cooled to room temperature, 25% (w / v) concentrated ammonia water was added to adjust the pH value to 10, followed by adding 10 mL of 1% (w / v) ascorbic acid aqueous solution and stirring evenly, and finally the reaction solution was allowed to stand at 25° C. for 6 h to allow the reaction to proceed fully to obtain a dispersion of silver nanosheets. The obtained dispersion of silver nanosheets was centrifuged at a speed of 8000 r / min, washed with deionized water, and finally dried at 80° C. for 4 h to obtain a powdered solid; the SEM image of the silver nanosheets is shown in FIG. Figure 6 As shown, the average particle size is between 100 and 200 nm.

[0096] In step 1 and step 2, the molecular structure of the gemini surfactant 16-4-16 is as shown below, wherein s=4.

[0097]

[0098] Example 7

[0099] A method for preparing size-adjustable silver nanosheets comprises the following steps:

[0100] Step 1, preparation of seed crystals:

[0101] First, 1 mL of 20% (w / v) AgNO3 aqueous solution was added to 9 mL of 3% (w / v) Gemini surfactant 16-4-16 aqueous solution under stirring, and then 2 mL of 20% (w / v) freshly prepared NaBH4 aqueous solution was added under vigorous stirring, and the mixture was allowed to stand for 2 h to obtain seed crystal A;

[0102] Step 2: Etching of seed crystal:

[0103] Then, 2 mL of seed A was added to 9 mL of 3% (w / v) aqueous solution of gemini surfactant 16-4-16, followed by 1 mL of 20% (w / v) AgNO3 aqueous solution, and the temperature was raised to 40°C and kept for 4 h to complete the etching of the seed. The obtained product was recorded as seed B.

[0104] Step 3: One-step growth of seed crystal:

[0105] After the obtained seed crystal B is cooled to room temperature, 25% (w / v) concentrated ammonia water is added to adjust the pH value to 11, and then 10 mL of 2% (w / v) ascorbic acid aqueous solution is added and stirred evenly. Finally, the reaction solution is allowed to stand at 25° C. for 14 h to allow the reaction to proceed fully, thereby obtaining a dispersion of silver nanosheets;

[0106] Step 4: Two-step growth of seed crystals:

[0107] 2 mL of the silver nanosheet dispersion prepared in step 3 was added to 9 mL of a 3% (w / v) aqueous solution of the gemini surfactant 16-4-16, followed by 1 mL of a 20% (w / v) aqueous solution of AgNO3, and then 25% (w / v) concentrated ammonia was added to adjust the pH value to 11, followed by 10 mL of a 2% (w / v) aqueous solution of ascorbic acid and stirring, and finally the reaction solution was allowed to stand at 25°C for 14 h to allow the reaction to proceed fully, and a dispersion of silver nanosheets was obtained again, the obtained dispersion of silver nanosheets was centrifuged at a speed of 200 r / min, washed with deionized water, and finally dispersed in water for storage; the SEM image of the silver nanosheets is shown in FIG. Figure 7 As shown, the average particle size is 2000nm.

[0108] In step 1, step 2 and step 4, the molecular structure of the gemini surfactant 16-4-16 is as shown below, wherein s=4.

[0109]

[0110] Example 8

[0111] A method for preparing size-adjustable silver nanosheets comprises the following steps:

[0112] Step 1, preparation of seed crystals:

[0113] First, 1 mL of 20% (w / v) AgNO3 aqueous solution was added to 9 mL of 4% (w / v) Gemini surfactant 16-4-16 aqueous solution under stirring, and then 2 mL of 20% (w / v) freshly prepared NaBH4 aqueous solution was added under vigorous stirring, and the mixture was allowed to stand for 2 h to obtain seed crystal A;

[0114] Step 2: Etching of seed crystal:

[0115] Then, 1 mL of seed A was added to 9 mL of 4% (w / v) aqueous solution of gemini surfactant 16-4-16, followed by 1 mL of 20% (w / v) AgNO3 aqueous solution, and the temperature was raised to 40°C and kept for 0.5 h to complete the etching of the seed. The obtained product was recorded as seed B.

[0116] Step 3: One-step growth of seed crystal:

[0117] After the obtained seed crystal B is cooled to room temperature, 25% (w / v) concentrated ammonia water is added to adjust the pH value to 11, and then 10 mL of 2% (w / v) ascorbic acid aqueous solution is added and stirred evenly. Finally, the reaction solution is allowed to stand at 25° C. for 14 h to allow the reaction to proceed fully, thereby obtaining a dispersion of silver nanosheets;

[0118] Step 4: Two-step growth of seed crystals:

[0119] 1 mL of the silver nanosheet dispersion prepared in step 3 was added to 9 mL of a 4% (w / v) aqueous solution of the gemini surfactant 16-4-16, followed by 1 mL of a 20% (w / v) aqueous solution of AgNO3, and then 25% (w / v) concentrated ammonia was added to adjust the pH value to 11, followed by 10 mL of a 2% (w / v) aqueous solution of ascorbic acid and stirring, and finally the reaction solution was allowed to stand at 25°C for 14 h to allow the reaction to proceed fully, and a dispersion of silver nanosheets was obtained again, the obtained dispersion of silver nanosheets was centrifuged at a speed of 200 r / min, washed with deionized water, and finally dispersed in water for storage; the SEM image of the silver nanosheets is shown in FIG. Figure 8 As shown, the average particle size is 3000nm.

[0120] In step 1, step 2 and step 4, the molecular structure of the gemini surfactant 16-4-16 is as shown below, wherein s=4.

[0121]

[0122] Example 9

[0123] A method for preparing size-adjustable silver nanosheets comprises the following steps:

[0124] Step 1, preparation of seed crystals:

[0125] First, 1 mL of 20% (w / v) AgNO3 aqueous solution was added to 9 mL of 3% (w / v) Gemini surfactant 16-10-16 aqueous solution under stirring, and then 2 mL of 20% (w / v) freshly prepared NaBH4 aqueous solution was added under vigorous stirring, and the mixture was allowed to stand for 2 h to obtain seed crystal A;

[0126] Step 2: Etching of seed crystal:

[0127] Then, 0.5 mL of seed A was added to 9 mL of 5% (w / v) aqueous solution of gemini surfactant 16-10-16, followed by 1 mL of 20% (w / v) AgNO3 aqueous solution, and the temperature was raised to 70°C and kept for 0.5 h to complete the etching of the seed. The obtained product was recorded as seed B.

[0128] Step 3: One-step growth of seed crystal:

[0129] After the obtained seed crystal B is cooled to room temperature, 25% (w / v) concentrated ammonia water is added to adjust the pH value to 11, and then 10 mL of 2% (w / v) ascorbic acid aqueous solution is added and stirred evenly. Finally, the reaction solution is allowed to stand at 25° C. for 14 h to allow the reaction to proceed fully, thereby obtaining a dispersion of silver nanosheets;

[0130] Step 4: Two-step growth of seed crystals:

[0131] 0.5 mL of the silver nanosheet dispersion prepared in step 3 was added to 9 mL of a 3% (w / v) aqueous solution of a gemini surfactant 16-10-16, followed by adding 1 mL of a 20% (w / v) aqueous solution of AgNO3, and then adding 25% (w / v) concentrated ammonia to adjust the pH value to 11, followed by adding 10 mL of a 2% (w / v) aqueous solution of ascorbic acid and stirring evenly, and finally the reaction solution was allowed to stand at 25°C for 14 h to allow the reaction to proceed fully to obtain a dispersion of silver nanosheets, the obtained dispersion of silver nanosheets was centrifuged at a speed of 200 r / min, washed with deionized water, and finally dried at 80°C for 24 h to obtain a powdered solid; the SEM image of the silver nanosheets is shown in FIG. Fig. 9 As shown, the average particle size is between 3000 and 5000 nm.

[0132] In step 1, step 2 and step 4, the molecular structure of the gemini surfactant 16-10-16 is as shown below, wherein s=10.

[0133]

[0134] In the present invention, the operations involved such as "vigorous stirring", "stirring", "centrifugation" and "washing" are routine operations in the field. As those skilled in the art should know, the degree of stirring of "vigorous stirring" is greater than that of "stirring".

[0135] In the present invention, the synthesis method of the quaternary ammonium salt surfactant is a method well known in the art. Zana reported the synthesis of quaternary ammonium salt surfactant in 1991 (Zana R, Benrraou M, Rueff R. Alkanediyl-.alpha.,.omega.-bis(dimethylalkylammonium bromide)surfactants.1. Effect of the spacerchain length on the critical micelle concentration and micelle ionization degree[J]. Langmuir, 1991, 7(6): 1072-1075), and the reaction equation is as shown in Formula II.

[0136]

[0137] Referring to the above synthesis method, the synthesis method of the gemini surfactant 16-10-16 is illustrated as follows: 24.8 g (92.2 mmol) of N, N-dimethylhexadecylamine is added to a 250 mL round-bottom flask, and then 100 mL of ethyl acetate is added as a solvent, and then 12.5 g (41.7 mmol) of 1,10-dibromodecane is added, and the mixture is refluxed for 48 hours under stirring. After cooling to room temperature, a white precipitate is precipitated, and the precipitate is collected by filtration. The obtained solid is redissolved in a mixed solvent of ethyl acetate (ethyl acetate) / ethanol and recrystallized 5 times. Finally, an oil pump is used to remove trace amounts of solvent to obtain a white powdery solid, which is the gemini surfactant 16-10-16. The reaction equation is shown in Formula III.

[0138]

[0139] The above embodiments and drawings do not limit the product form and style of the present invention. Any appropriate changes or modifications made by ordinary technicians in the relevant technical field should be deemed to be within the patent scope of the present invention.

Claims

1. A method for preparing size-adjustable silver nanosheets, characterized in that: The following steps are involved: Step 1, preparation of seed crystals: First, 1 mL of 5% to 50% (w / v) AgNO3 aqueous solution was added to 9 mL of 0.5% to 10% (w / v) gemini surfactant aqueous solution under stirring, and then 2 mL of 5% to 50% (w / v) freshly prepared NaBH4 aqueous solution was added under vigorous stirring, and the mixture was allowed to stand for 2 to 4 hours to obtain seed crystal A; Step 2: Etching of seed crystal: Then, 0.2-2 mL of seed crystal A was added to 9 mL of 0.5%-10% (w / v) aqueous solution of gemini surfactant, followed by 1 mL of 10%-50% (w / v) AgNO3 aqueous solution, and the temperature was raised to 40-70°C and kept for 0.5-4 h to complete the etching of the seed crystal. The obtained product was recorded as seed crystal B; Step 3: One-step growth of seed crystal: After the obtained seed crystal B is cooled to room temperature, concentrated ammonia is added to adjust the pH value to 8-11, and then 10 mL of 1%-10% (w / v) ascorbic acid aqueous solution is added and stirred evenly, and finally the reaction solution is allowed to stand at 25° C. for 1-14 hours to allow the reaction to proceed fully, thereby obtaining a dispersion of silver nanosheets, wherein the average particle size of the silver nanosheets is regulated within the range of 100-2000 nm; In step 1 and step 2, the gemini surfactant is a quaternary ammonium salt surfactant, and its molecular structure is shown in Formula I: Among them, when s=4, the gemini surfactant is recorded as 16-4-16, when s=6, the gemini surfactant is recorded as 16-6-16, and when s=10, the gemini surfactant is recorded as 16-10-16.

2. The method for preparing size-adjustable silver nanosheets according to claim 1, characterized in that: It also includes step 4, two-step growth of the seed crystal: 0.2-2 mL of the dispersion of silver nanosheets prepared in step 3 is added to 9 mL of an aqueous solution of 0.5%-10% (w / v) gemini surfactant, followed by adding 1 mL of an aqueous solution of 5%-50% (w / v) AgNO3, and then adding concentrated ammonia to adjust the pH value to 8-11, followed by adding 10 mL of an aqueous solution of 2%-10% (w / v) ascorbic acid and stirring evenly, and finally the reaction solution is allowed to stand at 25°C for 1-14 h to allow the reaction to proceed fully, to obtain a dispersion of silver nanosheets, the average particle size of which is regulated within the range of 2000-5000 nm.

3. The method for preparing size-adjustable silver nanosheets according to claim 2, characterized in that: In step 4, the gemini surfactant is a quaternary ammonium salt surfactant, and its molecular structure is shown in Formula I: Among them, when s=4, the gemini surfactant is recorded as 16-4-16, when s=6, the gemini surfactant is recorded as 16-6-16, and when s=10, the gemini surfactant is recorded as 16-10-16.

4. The method for preparing size-adjustable silver nanosheets according to claim 2, characterized in that: In step 4, the dispersion of the silver nanosheets obtained by the reaction is centrifuged, washed, and finally dispersed in water for storage; or dried at 80-100° C. for 4-24 hours to obtain a powdered solid.

5. The method for preparing size-adjustable silver nanosheets according to claim 1, characterized in that: In step 3, the concentration of the concentrated ammonia water is 25% to 28% (w / v).

6. The method for preparing size-adjustable silver nanosheets according to claim 1, characterized in that: In step 3, the dispersion of the silver nanosheets obtained by the reaction is centrifuged, washed, and finally dispersed in water for storage; or dried at 80-100° C. for 4-24 hours to obtain a powdered solid.

Citation Information

Patent Citations

  • Preparation method for flaky micro-aluminum powder

    CN101569936A

  • Preparation method for three-dimensional black nano metal wide-spectrum light absorption thin film

    CN106637356A

  • Preparation method of nanometer silver polyhedral quasi sphere

    CN106757373A

  • Chemical method for preparing nanoscale flaked silver powder

    CN107716944A

  • Method for preparing hierarchical-pore ZSM-5 molecular sieve by using anionic-nonionic gemini surfactant template

    CN110510634A