Preparation method of ultra-long silver nanowire

By using crystal nucleus inhibitors during the seed growth of silver nanowires, the length of silver nanowires is extended, and the problem of insufficient length of silver nanowires in the prior art is solved, and better conductivity and optical characteristics are achieved. High-performance transparent conductive film.

CN118905237AActive Publication Date: 2024-11-08QUANZHOU NORMAL UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410994403.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The prior art is difficult to prepare silver nanowires with longer lengths, resulting in limited electrical and optical characteristics, and it is impossible to effectively take into account the conductivity and light transmittance of transparent conductive films.

Method used

The seed growth method is adopted, and by adding a crystal nucleus inhibitor during the seed growth process, the formation of new crystal nucleus is prevented, and silver nitrate is promoted to adhere and reduce the existing silver nanowire seeds, extending the length of the silver nanowire, and preparing Extra-long silver nanowires with a length of 300 to 800 μm are produced.

Benefits of technology

The length of silver nanowires has been significantly improved, its conductivity and optical properties have been improved, and it can better take into account both conductivity and light transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905237A_ABST
    Figure CN118905237A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an ultra-long silver nanowire, which comprises the following steps of: adopting a seed crystal growth method, strictly controlling chemical reaction parameters, obtaining a silver nanowire which grows firstly, using the silver nanowire as a seed crystal, and growing a very long silver nanowire through a repeatedly improved growth process. According to the method, besides the innovation of the synthesis step of a seed crystal growth method, a crystal nucleus inhibitor for preventing formation of new crystal nucleuses, promoting continuous adhesion and reduction of silver nitrate on existing silver nanowire seed crystals and further causing continuous growth of the crystals is added in the seed crystal growth process, so that the length of the silver nanowires is greatly increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silver nanomaterials, and in particular to a method for preparing ultra-long silver nanowires. Background Art

[0002] Transparent conductive films (TCFs) are important components of devices such as tablets, readers, smart phones, touch screens, OLEDs, and organic solar cells. Silver nanowires (AgNWs) are one-dimensional metal materials. Due to their excellent electrical and thermal conductivity, good mechanical stability, and relatively acceptable price, AgNWs are considered to be the most promising raw material to replace ITO as the next generation of transparent conductive films, thus attracting widespread attention from many researchers. As far as current research is concerned, the properties of AgNWs are closely related to diameter, length, and dispersity. However, it is difficult to balance the light transmittance and conductivity of flexible transparent conductive films based on AgNWs. Therefore, in order to effectively solve the above problems, the research on batch preparation technology of AgNWs with higher aspect ratio has become a difficult problem that scientists have to overcome.

[0003] Existing studies have shown that the smoother the surface of AgNWs, the longer the length, the smaller the junction resistance between AgNWs, and the lower the sheet resistance of the AgNWs-based transparent conductor, the better the conductivity. The silver nanowires prepared by the prior art are relatively short, mostly in the range of 20 to 50 μm. For example, the preparation method of a high aspect ratio silver nanowire with publication number CN103537710A has a maximum length of 40 to 60 μm, so its electrical and optical properties are limited. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing ultra-long silver nanowires. The length of the prepared silver nanowires is extended to 300-800 μm, which greatly increases the length of the silver nanowires.

[0005] In order to achieve the above object, the solution of the present invention is:

[0006] A method for preparing ultra-long silver nanowires comprises the following steps:

[0007] Step 1, preparation of seed crystals:

[0008] S1. First, add 100 mL of ethylene glycol into a round-bottom flask at room temperature, and then add 0.08-2.4 g of PVP with an average molecular weight of 1,300,000 and 0.08-2.4 g of PVP with an average molecular weight of 40,000 to the ethylene glycol in sequence until they are completely dissolved to obtain a mixed solution;

[0009] S2, then add 0.08-2.4 g of silver nitrate to the mixed solution obtained in S1, and after it is completely dissolved, add 1-10 mL of 0.3-25 mM ethylene glycol solution of metal chloride to the mixed solution and stir for 1 min;

[0010] The metal chloride is one of NaCl, CuCl2 and FeCl3;

[0011] S3, then transfer the round-bottom flask containing the mixed solution obtained in S2 to an oil bath preheated to 110-170°C, stir for 10 min, stop stirring, react for 2-3 h, obtain seed crystals, and store them in an oven at 95°C for standby use;

[0012] Step 2: Preparation of crystal nucleus inhibitor:

[0013] Dissolve 0.1-0.2 g of surfactant in 50 mL of ethylene glycol / propylene glycol mixed solvent to obtain a crystal nucleation inhibitor for later use;

[0014] The surfactant is one of didodecyl dimethyl ammonium bromide, hexadecyl trimethyl ammonium bromide and didodecyl dimethyl ammonium bromide;

[0015] Step 3: Growth of seed crystals:

[0016] S1. Then 50 mL of ethylene glycol is added to the flask, and then the flask is suspended in an oil bath and heated under stirring, and 10 to 15 mL of a nucleus inhibitor is injected, followed by adding 0.08 to 2.4 g of PVP with an average molecular weight of 1,300,000 and 0.08 to 2.4 g of PVP with an average molecular weight of 40,000 and fully dissolving them uniformly, and then injecting 10 to 15 mL of the synthesized seed crystals, and then using a syringe pump to add 25 mL of AgNO3 solution at an injection rate of 0.5 to 2 mL / min. As the growth proceeds, the color of the reaction solution changes from bright ivory to opaque gray-green. After the silver nanowires are formed, the reaction is terminated by cooling the flask in a water bath at room temperature;

[0017] S2, then adding 100-500 mL of acetone solution to the synthesized silver nanowires to remove excess chemicals;

[0018] S3. The mixture obtained after impurity removal is then centrifuged to obtain a precipitate, which is finally redispersed in 100 to 500 mL of ethanol, centrifuged several times to wash the remaining PVP and other chemical substances, and finally dispersed in ethanol to obtain ultra-long silver nanowires with a length of 300 to 800 μm.

[0019] In S1 of step 1, the usage ratio of PVP with an average molecular weight of 1,300,000 to PVP with an average molecular weight of 40,000 is 1:2 to 2:1.

[0020] In step 2, the mass ratio of the ethylene glycol / propylene glycol mixed solvent is 2 to 1:1.

[0021] In S1 of step 3, the heating temperature is 110-170° C., and the concentration of the AgNO 3 solution is 0.32-9.6 g / 100 mL.

[0022] In S1 of step 3, the usage ratio of PVP with an average molecular weight of 1,300,000 to PVP with an average molecular weight of 40,000 is 1:2 to 2:1.

[0023] In S2 of step 3, the volume ratio of the acetone solution is 1:8-9.

[0024] After adopting the above technical scheme, the present invention provides a method for preparing ultra-long silver nanowires. By adopting the seed growth method, the chemical reaction parameters are strictly controlled to obtain the first grown silver nanowires, which are used as seeds, and then very long silver nanowires are grown by repeating the improved growth process. However, simply adding chemical substances and simply repeating the conventional silver nanowire growth process cannot achieve the growth of longer silver nanowires, but will produce many byproduct nanoparticles. In addition to the innovation of the synthesis step of the seed growth method, the method of the present invention also adds a nucleus inhibitor in the process of seed growth to prevent the formation of new crystal nuclei, promote silver nitrate to continue to attach and reduce to the existing silver nanowire seed crystals, and then cause the crystals to continue to grow, thereby greatly increasing the length of the silver nanowires. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a SEM image of the ultra-long silver nanowires prepared in Example 1;

[0026] Figure 2 This is a SEM image of the ultra-long silver nanowires prepared in Example 2;

[0027] Figure 3 This is a SEM image of the ultra-long silver nanowires prepared in Example 3;

[0028] Figure 4 This is the SEM image of the silver nanowires prepared in the comparative example. DETAILED DESCRIPTION

[0029] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.

[0030] Example 1

[0031] A method for preparing ultra-long silver nanowires comprises the following steps:

[0032] Step 1, preparation of seed crystals:

[0033] S1. First, add 100 mL of ethylene glycol into a round-bottom flask at room temperature, and then add 1.2 g of PVP with an average molecular weight of 1,300,000 and 1.6 g of PVP with an average molecular weight of 40,000 to the ethylene glycol in sequence until they are completely dissolved to obtain a mixed solution;

[0034] S2, then add 1.2g of silver nitrate to the mixed solution obtained in S1, and after it is completely dissolved, add 10mL of 12mMFeCl3 ethylene glycol solution to the mixed solution and stir for 1min;

[0035] S3, then transfer the round-bottom flask containing the mixed solution obtained in S2 to an oil bath preheated to 170°C, stir for 10 minutes, stop stirring, react for 3 hours, obtain seed crystals, and store them in an oven at 95°C for standby use;

[0036] Step 2: Preparation of crystal nucleus inhibitor:

[0037] Dissolve 0.1 g of didodecyl dimethyl ammonium bromide in 50 mL of a 2:1 ethylene glycol / glycerol mixed solvent to obtain a crystal nucleus inhibitor for later use;

[0038] Step 3: Growth of seed crystals:

[0039] S1. Then, 50 mL of ethylene glycol was added to a clean flask, and the flask was suspended in an oil bath and heated to 130°C under continuous magnetic stirring. 10 mL of a nucleus inhibitor was injected, and then 1.2 g of PVP with an average molecular weight of 1,300,000 and 1.6 g of PVP with an average molecular weight of 40,000 were added to the above ethylene glycol in sequence until they were completely dissolved. Then, 15 mL of the synthesized seed crystals were injected, and then 25 mL of 1.2 g / 100 mL AgNO3 solution was added at an injection rate of 1 mL / min using a syringe pump. As the growth progressed, the color of the reaction solution changed from bright ivory to opaque gray-green. After the silver nanowires were formed, the reaction was terminated by cooling the flask in a water bath at room temperature.

[0040] S2, then adding 400 mL of acetone solution with a volume fraction of 1:9 to the synthesized silver nanowires to remove excess chemicals such as ethylene glycol and PVP;

[0041] S3. The mixture obtained after impurity removal is then centrifuged to obtain a precipitate, which is redispersed in 200 mL of ethanol and centrifuged several times to wash the remaining PVP and other chemical substances, and finally dispersed in ethanol to obtain ultra-long silver nanowires with a length of 300 to 500 μm. The SEM image of the silver nanowires is shown in FIG. Figure 1 shown.

[0042] Example 2

[0043] A method for preparing ultra-long silver nanowires comprises the following steps:

[0044] Step 1, preparation of seed crystals:

[0045] S1. First, add 100 mL of ethylene glycol into a round-bottom flask at room temperature, and then add 0.16 g of PVP with an average molecular weight of 1,300,000 and 0.08 g of PVP with an average molecular weight of 40,000 to the ethylene glycol in sequence until they are completely dissolved to obtain a mixed solution;

[0046] S2, then add 0.24g of silver nitrate to the mixed solution obtained in S1, and after it is completely dissolved, add 1mL of 2mM CuCl2 ethylene glycol solution to the mixed solution and stir for 1min;

[0047] S3, then transfer the round-bottom flask containing the mixed solution obtained in S2 to an oil bath preheated to 150° C., stir for 10 min, stop stirring, react for 3 h, obtain seed crystals, and store them in an oven at 95° C. for standby use;

[0048] Step 2: Preparation of crystal nucleus inhibitor:

[0049] Dissolve 0.2 g of hexadecyltrimethylammonium bromide in 50 mL of a 1:1 ethylene glycol / glycerol mixed solvent to obtain a crystal nucleus inhibitor for later use;

[0050] Step 3: Growth of seed crystals:

[0051] S1. Then, 50 mL of ethylene glycol was added to a clean flask, which was then suspended in an oil bath and heated to 150°C under continuous magnetic stirring. 10 mL of a nucleus inhibitor was injected, followed by the addition of 0.16 g of PVP with an average molecular weight of 1,300,000 and 0.08 g of PVP with an average molecular weight of 40,000 to the above ethylene glycol until completely dissolved, followed by the injection of 15 mL of the synthesized seed crystals, followed by the use of a syringe pump to add 25 mL of a 0.64 g / 100 mL AgNO3 solution at an injection rate of 1 mL / min. As the growth proceeded, the color of the reaction solution changed from bright ivory to opaque gray-green. After the silver nanowires were formed, the reaction was terminated by cooling the flask in a water bath at room temperature.

[0052] S2, then adding 500 mL of acetone solution with a volume fraction of 1:9 to the synthesized silver nanowires to remove excess chemicals such as ethylene glycol and PVP;

[0053] S3. The mixture obtained after impurity removal is then centrifuged to obtain a precipitate, which is redispersed in 200 mL of ethanol and centrifuged several times to wash the remaining PVP and other chemical substances, and finally dispersed in ethanol to obtain ultra-long silver nanowires with a length of 500 to 800 μm. The SEM image of the silver nanowires is shown in FIG. Figure 2 shown.

[0054] Example 3

[0055] A method for preparing ultra-long silver nanowires comprises the following steps:

[0056] Step 1, preparation of seed crystals:

[0057] S1. First, add 100 mL of ethylene glycol into a round-bottom flask at room temperature, and then add 0.42 g of PVP with an average molecular weight of 1,300,000 and 0.84 g of PVP with an average molecular weight of 40,000 to the ethylene glycol in sequence until they are completely dissolved to obtain a mixed solution;

[0058] S2, then add 0.56g of silver nitrate to the mixed solution obtained in S1, and after it is completely dissolved, add 5mL of 2mM NaCl ethylene glycol solution to the mixed solution and stir for 1min;

[0059] S3, then transfer the round-bottom flask containing the mixed solution obtained in S2 to an oil bath preheated to 170°C, stir for 10 minutes, stop stirring, react for 2.5 hours, obtain seed crystals, and store them in an oven at 95°C for standby use;

[0060] Step 2: Preparation of crystal nucleus inhibitor:

[0061] Dissolve 0.1 g of dihexadecyl dimethyl ammonium bromide in 50 mL of a 1:1 ethylene glycol / glycerol mixed solvent to obtain a crystal nucleus inhibitor for later use;

[0062] Step 3: Growth of seed crystals:

[0063] S1. Then, 50 mL of ethylene glycol was added to a clean flask, and the flask was suspended in an oil bath and heated to 170°C under continuous magnetic stirring. 10 mL of a nucleus inhibitor was injected, and then 0.64 g of PVP with an average molecular weight of 1,300,000 and 0.32 g of PVP with an average molecular weight of 40,000 were added to the above ethylene glycol in sequence until they were completely dissolved, and then 15 mL of the synthesized seed was injected, and then 25 mL of 1.2 g / 100 mL AgNO3 solution was added at an injection rate of 0.5 mL / min using a syringe pump. As the growth progressed, the color of the reaction solution changed from bright ivory to opaque gray-green. After the silver nanowires were formed, the reaction was terminated by cooling the flask in a water bath at room temperature.

[0064] S2, then adding 400 mL of acetone solution with a volume fraction of 1:8 to the synthesized silver nanowires to remove excess chemicals such as ethylene glycol and PVP;

[0065] S3. The mixture obtained after impurity removal is then centrifuged to obtain a precipitate, which is redispersed in 200 mL of ethanol and centrifuged several times to wash the remaining PVP and other chemical substances, and finally dispersed in ethanol to obtain ultra-long silver nanowires with a length of 300 to 500 μm. The SEM image of the silver nanowires is shown in FIG. Figure 3 shown.

[0066] Comparative Example

[0067] A method for preparing silver nanowires comprises the following steps:

[0068] Step 1, preparation of seed crystals:

[0069] S1. First, add 100 mL of ethylene glycol into a round-bottom flask at room temperature, and then add 1.2 g of PVP with an average molecular weight of 1,300,000 and 1.6 g of PVP with an average molecular weight of 40,000 to the ethylene glycol in sequence until they are completely dissolved to obtain a mixed solution;

[0070] S2, then add 1.2g of silver nitrate to the mixed solution obtained in S1, and after it is completely dissolved, add 10mL of 12mMFeCl3 ethylene glycol solution to the mixed solution and stir for 1min;

[0071] S3, then transfer the round-bottom flask containing the mixed solution obtained in S2 to an oil bath preheated to 170°C, stir for 10 minutes, stop stirring, react for 3 hours, obtain seed crystals, and store them in an oven at 95°C for standby use;

[0072] Step 2: Growth of seed crystals:

[0073] S1. Then, 50 mL of ethylene glycol was added to a clean flask, and the flask was suspended in an oil bath and heated to 130°C under continuous magnetic stirring. Then, 1.2 g of PVP with an average molecular weight of 1,300,000 and 1.6 g of PVP with an average molecular weight of 40,000 were added to the above ethylene glycol in sequence until they were completely dissolved. Then, 15 mL of the synthesized seed crystals were injected, and then 25 mL of 1.2 g / 100 mL AgNO3 solution was added at an injection rate of 1 mL / min using a syringe pump. As the growth progressed, the color of the reaction solution changed from bright ivory to opaque grayish white. After the silver nanowires were formed, the reaction was terminated by cooling the flask in a water bath at room temperature.

[0074] S2, then adding 400 mL of acetone solution with a volume fraction of 1:9 to the synthesized silver nanowires to remove excess chemicals such as ethylene glycol and PVP;

[0075] S3, the mixture obtained after impurity removal is then centrifuged to obtain a precipitate, which is redispersed in 200 mL of ethanol, centrifuged several times to wash the remaining PVP and other chemicals, and finally dispersed in ethanol to obtain silver nanowires with a length of less than 50 μm. The SEM image of the silver nanowires is shown in FIG. Figure 4 shown.

[0076] The reagents used in the present invention are all commercially available reagents.

[0077] The above embodiments and drawings do not limit the product form and style of the present invention. Any appropriate changes or modifications made by ordinary technicians in the relevant technical field should be deemed to be within the patent scope of the present invention.

Claims

1. A method for preparing ultra-long silver nanowires, characterized in that: The following steps are involved: Step 1, preparation of seed crystals: S1. First, add 100 mL of ethylene glycol into a round-bottom flask at room temperature, and then add 0.08-2.4 g of PVP with an average molecular weight of 1,300,000 and 0.08-2.4 g of PVP with an average molecular weight of 40,000 to the ethylene glycol in sequence until they are completely dissolved to obtain a mixed solution; S2, then add 0.08-2.4 g of silver nitrate to the mixed solution obtained in S1, and after it is completely dissolved, add 1-10 mL of 0.3-25 mM ethylene glycol solution of metal chloride to the mixed solution and stir for 1 min; The metal chloride is one of NaCl, CuCl2 and FeCl3; S3, then transfer the round-bottom flask containing the mixed solution obtained in S2 to an oil bath preheated to 110-170° C., stir for 10 min, stop stirring, react for 2-3 h, obtain seed crystals, and store them in an oven for later use; Step 2: Preparation of crystal nucleus inhibitor: Dissolve 0.1-2 g of surfactant in 50 mL of ethylene glycol / propylene glycol mixed solvent to obtain a crystal nucleation inhibitor for later use; The surfactant is one of didodecyl dimethyl ammonium bromide, hexadecyl trimethyl ammonium bromide and didodecyl dimethyl ammonium bromide; Step 3: Growth of seed crystals: S1. Then 50 mL of ethylene glycol is added to the flask, and then the flask is suspended in an oil bath, heated under stirring, and 10 to 15 mL of a nucleus inhibitor is injected, followed by adding 0.08 to 2.4 g of PVP with an average molecular weight of 1,300,000 and 0.08 to 2.4 g of PVP with an average molecular weight of 40,000 and fully dissolving them uniformly, and then injecting 10 to 15 mL of the synthesized seed crystals, and then using a syringe pump to add 25 mL of AgNO3 solution at an injection rate of 0.5 to 2 mL / min. As the growth proceeds, after the silver nanowires are formed, the reaction is terminated by cooling the flask in a water bath at room temperature; S2, then adding 100-500 mL of acetone solution to the synthesized silver nanowires to remove excess chemicals; S3. The mixture obtained after impurity removal is then centrifuged to obtain a precipitate, which is redispersed in 100 to 500 mL of ethanol, centrifuged several times to wash the remaining chemical substances, and finally dispersed in ethanol to obtain ultra-long silver nanowires with a length of 300 to 800 μm.

2. The method for preparing ultra-long silver nanowires according to claim 1, characterized in that: In S1 of step 1, the usage ratio of PVP with an average molecular weight of 1,300,000 to PVP with an average molecular weight of 40,000 is 1:2 to 2:

1.

3. The method for preparing ultra-long silver nanowires according to claim 1, characterized in that: In step 2, the mass ratio of the ethylene glycol / propylene glycol mixed solvent is 2 to 1:

1.

4. The method for preparing ultra-long silver nanowires according to claim 1, characterized in that: In S1 of step 3, the heating temperature is 110-170° C., and the concentration of the AgNO 3 solution is 0.32-9.6 g / 100 mL.

5. The method for preparing ultra-long silver nanowires according to claim 1, characterized in that: In S1 of step 3, the usage ratio of PVP with an average molecular weight of 1,300,000 to PVP with an average molecular weight of 40,000 is 1:2 to 2:

1.

6. The method for preparing ultra-long silver nanowires according to claim 1, characterized in that: In S2 of step 3, the volume ratio of the acetone solution is 1:8-9.

Citation Information

Patent Citations

  • Preparing method of ultra-long silver nanowire

    CN103433503A

  • Preparation method of ultrahigh length-diameter ratio nanometer silver thread

    CN108856726A

  • Continuous flow production of metal nanowires

    CN111225755A

  • Mass Production Method of Ag NanoWire

    KR1020120010198A

  • Method for continuously fabricating silver nanowire

    US20100242679A1