Welding method for large-diameter large-thickness high-strength steel spherical end socket

By using an X-shaped bevel with blunt edges and a multi-layer, multi-pass welding method, combined with trolley rails and shielded gas welding technology, the problems of low welding efficiency, unstable quality, and large deformation of large-diameter, thick, and high-strength steel spherical heads were solved, achieving efficient, aesthetically pleasing, and stable welding results.

CN118905391APending Publication Date: 2024-11-08WUCHANG SHIPBUILDING INDUSTRY GROUP CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411175401.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing technology for welding large-diameter, thick, high-strength steel spherical heads has low welding efficiency, unstable quality, poor appearance, large welding deformation and easy weld breakage, and there is also the problem of cracking in the tack weld.

Method used

The X-shaped bevel with blunt edge is used, combined with multi-layer and multi-pass welding method and trolley track. The welding trolley performs tack welding, bottom sealing welding, and welding of the outer and inner parts of the tile. Arc welding is performed using argon-rich and carbon dioxide mixed gas shielding gas. The trolley is used in conjunction with plasma cleaning trolley and magnetic trolley track for cleaning and correction.

Benefits of technology

It improves welding efficiency, ensures the stability and aesthetics of welding quality, reduces welding deformation, lowers the labor intensity of welders, and prevents tack weld cracking caused by welding deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905391A_ABST
    Figure CN118905391A_ABST
Patent Text Reader

Abstract

The invention relates to a welding method of a large-diameter and large-thickness high-strength steel spherical head, which comprises the following steps of: processing an arc-shaped plate and a top cover plate into an X-shaped groove, and performing positioned welding; the inner side part of the X-shaped groove is subjected to bottom sealing welding; the outer side parts of the X-shaped grooves are welded, specifically, a multi-layer and multi-pass welding method is adopted, the outer side parts, between adjacent arc-shaped plates and between adjacent top cover plates, of the X-shaped grooves are welded through a welding trolley, and the outer side parts are filled to be lower than the outer wall faces of tiles by a first preset distance; a magnetic attraction trolley track is arranged to be circular, a multi-layer and multi-pass welding method is adopted, the outer side part of the X-shaped groove between the arc-shaped plate and the top cover plate is welded through a welding trolley, and the outer side part of the X-shaped groove is filled to be lower than the outer wall face of the tile by a first preset distance; welding the inner side part of the X-shaped groove so as to fill the inner side part of the X-shaped groove to be lower than the outer wall surface of the tile by a first preset distance; and the inner side part and the outer side part of the X-shaped groove are welded to form a capping layer. The welding device is high in welding efficiency, good in quality and good in appearance forming.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of spherical head manufacturing, and in particular to a welding method for a large-diameter, large-thickness, high-strength steel spherical head. Background Art

[0002] See also Figure 1 and Figure 2 As shown, the existing spherical head is made of high-strength steel, with a port diameter of more than 6 meters and a plate thickness of about 50 mm. Due to the limitation of processing capacity, it cannot be pressed and formed at one time, so it is welded by twelve tiles. The twelve tiles include ten arc-shaped plates 1 and two top cover plates 2, wherein a first vertical rotation flat weld 3 is formed between two adjacent pieces of the ten arc-shaped plates 1, with a total of ten, a second vertical rotation flat weld 4 is formed between the two top cover plates 2, with a total of one, and an annular weld 5 is formed between the ten arc-shaped plates 1 and the two top cover plates 2, with a total of twelve welds, wherein the intersection of the annular weld 5 and the first vertical rotation flat weld 3 forms a T-joint 6 by the groove before welding.

[0003] The original manufacturing method uses a Y-shaped groove and multi-person manual arc welding. This manufacturing method has many disadvantages, such as:

[0004] (1) The manual arc welding has low welding efficiency and long welding cycle, unstable welding quality, poor weld appearance, large welding deformation, easy weld collapse, poor overall dimensional accuracy, and there is also the problem of positioning weld cracking caused by welding deformation.

[0005] (2) Because the welding gun is in the middle of the trolley, when welding the T-joint weld, there is a problem of how the welding trolley passes the groove.

[0006] (3) The root cleaning work on the back of the weld is generally carried out by manual carbon arc gouging. The root cleaning straightness and width are poor, and the dimensional accuracy is poor, resulting in unsightly weld formation. Summary of the invention

[0007] The embodiment of the present application provides a welding method for a large-diameter, large-thickness, high-strength steel spherical head to solve the problems of low efficiency and long welding cycle, unstable welding quality, poor weld appearance, large welding deformation, easy weld collapse, poor overall dimensional accuracy, and positioning weld cracking caused by welding deformation using manual arc welding in the related art.

[0008] The embodiment of the present application provides a welding method for a large-diameter, large-thickness, high-strength steel spherical head, which comprises:

[0009] Beveling all tiles to form an X-shaped bevel with a blunt edge, wherein all tiles include a curved plate and a top cover plate;

[0010] On the tire frame, positioning welding is performed on all the tiles;

[0011] Performing back-welding on the inner side of the X-shaped groove to form a back-weld bead;

[0012] Make the opening of the spherical head face downward and weld the outer part of the X-shaped groove, including:

[0013] - Using a multi-layer and multi-pass welding method, the outer portion of the X-shaped groove between adjacent arc-shaped plates and adjacent top cover plates is welded by a welding carriage to fill the groove to a first preset distance L1 below the outer wall surface of the tile;

[0014] - Arrange the magnetic trolley track into a circle to cover all the arc-shaped plates, and adopt a multi-layer and multi-pass welding method to weld the outer part of the X-shaped groove between the arc-shaped plate and the top cover plate through the welding trolley to fill it to a first preset distance L1 below the outer wall of the tile;

[0015] After cutting with the tire frame, the inner part of the X-shaped groove is cleaned;

[0016] The opening of the spherical head is facing upward, and the inner part of the X-shaped groove is welded to fill it to a first preset distance L1 below the outer wall of the tile;

[0017] The inner and outer portions of the X-shaped groove are welded to form a capping layer.

[0018] In some embodiments, positioning welding is performed on all the tiles on the tire frame, specifically including:

[0019] Assemble on the tire frame according to the shape of the spherical head;

[0020] Spot welding each of the tiles to fix them on the tire frame;

[0021] Along the extension direction of the X-shaped groove between the adjacent arc-shaped plates, an arc-starting plate is welded at the end of the X-shaped groove between the adjacent arc-shaped plates, so as to facilitate the welding trolley to travel when starting the arc;

[0022] The spot welding comprises: using a mixed gas of rich argon and carbon dioxide as a shielding gas and adopting a solid welding wire in combination with arc welding to perform welding.

[0023] In some embodiments, the positioning welding and the backing welding both include preheating before welding and post-heating after welding, the preheating temperature is 120-140° C., and the post-heating temperature is 220-240° C.;

[0024] And / or, the steps for welding the inner portion of the X-shaped groove are the same as those for welding the outer portion of the X-shaped groove.

[0025] In some embodiments, welding the outer portion of the X-shaped groove between adjacent arc-shaped plates to fill the groove to a first preset distance L1 below the outer wall of the tile specifically includes:

[0026] Arrange the X-shaped grooves between the adjacent arc-shaped plates in sequence and divide them into two sequence groups, namely an odd-numbered sequence group and an even-numbered sequence group;

[0027] Drive the welding carriage to move from bottom to top along the extension direction of the X-shaped groove, and synchronously weld the outer portions of each X-shaped groove in one sequence group to fill the groove to a second preset distance L2 below the outer wall of the tile;

[0028] Drive the welding carriage to move from bottom to top along the extension direction of the X-shaped groove, and then synchronously weld the outer parts of each X-shaped groove in another sequence group to fill it to a first preset distance L1 below the outer wall of the tile, L1<L2;

[0029] The filling is continued so that the second preset distance L2 is reduced to the first preset distance L1.

[0030] In some embodiments, the second preset distance L2 is two-thirds of the depth of the outer portion of the X-shaped groove;

[0031] And / or, the first preset distance L1 is 0-1 mm;

[0032] And / or, the arc closing point of each welding carriage is located in the X-shaped groove between the arc plate and the top cover plate.

[0033] In some embodiments, welding the outer portions of the X-shaped grooves between adjacent top cover plates to fill the grooves to a first preset distance L1 below the outer wall of the tile specifically includes:

[0034] Along the extension direction of the X-shaped groove, a welding carriage is arranged at both ends of the top cover plate;

[0035] Driving two welding carriages to move toward each other and perform welding to fill the gap to a first preset distance L1 below the outer wall of the tile;

[0036] The arc starting times of the two welding carriages are separated by a preset time.

[0037] In some embodiments, the arc starting point of each welding carriage is located in the X-shaped groove between the arc plate and the top cover plate.

[0038] In some embodiments, the outer portion of the X-shaped groove between the arc plate and the top cover plate is welded to fill the outer portion to a first preset distance L1 below the outer wall surface of the tile, specifically comprising:

[0039] Arrange multiple welding trolleys at equal distances along the circumference of the magnetic trolley track;

[0040] The welding carriages are driven to move synchronously and in the same direction, and welding is performed to fill the gap to a first preset distance L1 below the outer wall of the tile.

[0041] In some embodiments, the arc starting point and arc ending point of each welding carriage are staggered from the T-joint, and the T-joint is formed at the intersection of the X-shaped groove between adjacent arc plates and the X-shaped groove between the arc plate and the top cover plate.

[0042] In some embodiments, the inner portion of the X-shaped groove is cleaned, specifically comprising:

[0043] According to the order of cleaning the X-shaped grooves between the adjacent arc plates, between the adjacent top cover plates, and then the X-shaped grooves between the arc plates and the top cover plates, the air planer is first used to clean the grooves so that the inner part of each X-shaped groove has the same depth, and then the plasma cleaning trolley is used in conjunction with the magnetic trolley track to correct and straighten the inner part of the X-shaped groove;

[0044] Finally, polish it clean to reveal the metallic luster of the carbonized layer.

[0045] The beneficial effects of the technical solution provided by this application include:

[0046] Compared with manual arc welding, this application has high welding efficiency, beautiful shape, stable quality, small deformation, and low labor intensity for welders; by using an X-shaped groove with a blunt edge, the bottom is sealed and welded before welding to prevent positioning weld cracking caused by welding deformation.

[0047] The use of trolley rails and other tooling and a reasonable welding sequence can solve the problem of over-welding of T-joints when welding with a welding trolley and reduce welding blind areas.

[0048] The use of manual planing and plasma gouging can ensure that defects are cleaned up and the root straightness and accuracy are guaranteed, which is beneficial to welding. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0050] Figure 1 A schematic diagram of a spherical head provided for this application from one perspective;

[0051] Figure 2A schematic diagram of another perspective of the spherical head provided for this application;

[0052] Figure 3 Schematic diagram of X-shaped groove provided for this application;

[0053] Figure 4 The bottom seal welding diagram provided for this application;

[0054] Figure 5 A schematic diagram of a sequential group welding of the outer portion of the X-shaped groove between adjacent curved plates provided in the present application;

[0055] Figure 6 A schematic diagram of another sequential group welding of the outer portion of the X-shaped groove between adjacent curved plates provided in the present application;

[0056] Figure 7 A schematic diagram of the outer portion of the X-shaped groove provided in the present application being filled to a second preset distance below the outer wall of the tile;

[0057] Figure 8 A schematic diagram of the outer portion of the X-shaped groove provided in the present application being filled to a first preset distance below the outer wall surface of the tile;

[0058] Fig. 9 A schematic diagram of the arc closing point position provided for this application;

[0059] Fig.10 Schematic diagram of welding trolley provided for this application;

[0060] Fig.11 A schematic diagram of the track layout of the magnetic trolley provided for this application;

[0061] Fig.12 A schematic diagram of welding the outer portion of the X-shaped groove between adjacent top cover plates provided in this application;

[0062] Fig.13 A schematic diagram of the welding of the outer portion of the X-shaped groove between the curved plate and the top cover plate provided in this application;

[0063] Fig.14 A schematic diagram of a spherical head with the opening facing upward provided in this application;

[0064] Fig.15 A schematic diagram of cleaning the inner part of an X-shaped groove provided for this application;

[0065] Fig.16 A schematic diagram of the welding of the inner side of the X-shaped groove between adjacent top cover plates provided in this application;

[0066] Fig.17 A schematic diagram of the inner part of the X-shaped groove provided in the present application being filled to a first preset distance below the inner wall surface of the tile;

[0067] Fig.18 A schematic diagram of a sequential group welding of the inner side portion of the X-shaped groove between adjacent curved plates provided in the present application;

[0068] Fig.19 Another schematic diagram of welding of the inner side of the X-shaped groove between adjacent curved plates provided in the present application;

[0069] Fig. 20 Schematic diagram of cover layer welding provided for this application.

[0070] In the figure: 1. Arc plate; 2. Top cover plate; 3. First vertical flat weld; 4. Second vertical flat weld; 5. Annular weld; 6. T-joint; 7. Inner part; 8. Outer part; 9. Bottom weld; 10. Welding trolley; 11. Magnetic trolley track; 12. Cover layer; 13. Arc closing point; 14. Stainless steel plate. DETAILED DESCRIPTION

[0071] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0072] The embodiment of the present application provides a welding method for a large-diameter, large-thickness, high-strength steel spherical head, which comprises the following steps:

[0073] 101: After all the tiles are pressed linearly, all the tiles are beveled to form an X-shaped bevel with a blunt edge, such as Figure 3 As shown, the X-shaped groove includes an outer portion 8 located outside the spherical head and an inner portion 7 located inside the spherical head. As an example, the angle β of the outer portion 8 is smaller than the angle θ of the inner portion 7. The angle β is 62-65° and the angle θ is 100-120°. The thickness d1 of the blunt edge and the depth d2 of the outer portion 8 can be determined according to actual needs. As an example, the thickness d1 of the blunt edge is 7mm and the depth d2 of the outer portion 8 is 32-36mm. When using a milling machine for processing, the dimensional accuracy of the groove is ensured. All of the tiles include a curved plate 1 and a top cover plate 2; for example Figure 1 Among them, there are ten curved plates 1 and two top cover plates 2.

[0074] 102: On the tire frame, all the tiles are tack welded.

[0075] Specifically, step 102 can be operated as follows: assemble on the tire frame according to the shape of the spherical head; then spot weld each tile to fix it on the tire frame; finally, weld an arc-starting plate at the end of the X-shaped groove between the adjacent arc plates 1 along the extension direction of the X-shaped groove between the adjacent arc plates 1, so that the welding trolley 10 can travel when the arc is started, that is, the arc-starting plate is welded at the opening of the spherical head, and then the X-shaped groove between the adjacent arc plates 1 is welded. When the arc is started, the welding trolley 10 travels on the arc-starting plate, and no blind area for the trolley welding is formed. The line shape of the arc-starting plate is consistent with the line shape of the arc plate 1.

[0076] The spot welding comprises: using a mixed gas of rich argon and carbon dioxide as a shielding gas and adopting a solid welding wire in combination with arc welding to perform welding.

[0077] The advantages of using gas shielded welding are high current density, concentrated arc heat and gas cooling, which reduces welding deformation. Solid welding wire is used with a mixture of argon-rich and carbon dioxide as the shielding gas, and TPS500i welding power source is used for welding. The arc is stable and spatter is small. The spherical head is installed and positioned on the tire frame with the opening facing downward, and is spot-welded to the tire frame, which plays a role in rigid fixation and reduces welding deformation.

[0078] 103: See Figure 4 As shown, the inner portion 7 of the X-shaped groove is subjected to bottom welding to form a bottom weld bead 9.

[0079] Before the formal welding, the bottom welding inside the spherical head is carried out first. The purpose is to improve the strength of the positioning weld and prevent the positioning weld from cracking and exploding due to deformation or excessive stress during the formal welding.

[0080] The positioning welding and the backing welding both include preheating before welding and post-heating after welding, the preheating temperature is 120-140°C, the post-heating temperature is 220-240°C, and the welding is cooled naturally to room temperature. Both preheating and post-heating are performed using electromagnetic induction heating equipment.

[0081] 104: The opening of the spherical head is directed downward, and the outer portion 8 of the X-shaped groove is welded, specifically including:

[0082] Combination Figure 5 , Figure 6 , Figure 7 , Figure 8 , Fig. 9 , Fig.10 , Fig.11 and Fig.12As shown, a multi-layer multi-pass welding method is adopted, and the outer part 8 of the X-shaped groove between the adjacent arc-shaped plates 1 is welded by the welding trolley 10 to fill it to a distance lower than the first preset distance L1 of the outer wall of the tile, and the outer part 8 of the X-shaped groove between the adjacent top cover plates 2 is welded to fill it to a distance lower than the first preset distance L1 of the outer wall of the tile; the magnetic trolley track 11 is arranged in a circle to cover all the arc-shaped plates 1, and a multi-layer multi-pass welding method is adopted, and the outer part 8 of the X-shaped groove between the arc-shaped plate 1 and the top cover plate 2 is welded by the welding trolley 10 to fill it to a distance lower than the first preset distance L1 of the outer wall of the tile;

[0083] 105: After cutting with the tire frame, the inner part 7 of the X-shaped groove is cleaned.

[0084] 106: Make the opening of the spherical head face upwards, and weld the inner part 7 of the X-shaped groove to fill it to a first preset distance L1 below the outer wall of the tile.

[0085] 107: The inner part 7 and the outer part 8 of the X-shaped groove are welded to form a cover layer 12.

[0086] In step 107, after the cap layer 12 is welded, the X-shaped groove between the two adjacent curved plates 1 forms a first vertical-to-flat weld 3, the X-shaped groove between the two top cover plates 2 forms a second vertical-to-flat weld 4, and the X-shaped groove between the curved plate 1 and the top cover plate 2 forms a circular weld 5. Figure 1 and Figure 2 shown.

[0087] Wherein, in step 104, the outer portion 8 of the X-shaped groove between the adjacent arc-shaped plates 1 is welded to fill the groove to a first preset distance L1 below the outer wall of the tile, which specifically includes the following steps:

[0088] 201: Arrange the X-shaped grooves between the adjacent arc-shaped plates 1 in sequence and divide them into two sequence groups, namely an odd-numbered sequence group and an even-numbered sequence group.

[0089] for example, Figure 5 There are ten curved plates 1, which are divided into two serial groups, each with five. The odd serial group includes the curved plates 1 with serial numbers of one, three, five, seven and nine, and the even serial group includes the curved plates 1 with serial numbers of two, four, six, eight and ten.

[0090] 202: See Figure 5 , Figure 7 As shown, Figure 5The middle arrow indicates the moving direction of the welding carriage 10. The welding carriage 10 is driven to move from bottom to top along the extension direction of the X-shaped groove, and the outer parts 8 of each X-shaped groove in one of the sequence groups are welded synchronously to fill it to a second preset distance L2 below the outer wall of the tile.

[0091] Since the opening of the spherical head faces downward, when welding is performed, the direction from bottom to top is from the opening side of the spherical head toward the top cover plate 2.

[0092] The welding carriage 10 in step 202 moves synchronously to weld the X-shaped groove of one sequence group at a time, and first fills it to the second preset distance L2, in order to prevent excessive welding deformation and insufficient overall strength of the spherical wall from causing desoldering and uneven deformation problems when welding another sequence group.

[0093] 203: See Figure 6 and Figure 8 As shown, Figure 6 The middle arrow indicates the moving direction of the welding trolley 10, which is driven to move from bottom to top along the extension direction of the X-shaped groove, and then the outer parts 8 of each X-shaped groove in another sequence group are welded synchronously to fill it to a first preset distance L1 below the outer wall of the tile, L1<L2.

[0094] 204: See Figure 8 As shown, the X-shaped groove of the previous sequence group continues to be filled so that the second preset distance L2 is reduced to the first preset distance L1.

[0095] See also Fig. 9 As shown, in the above steps 202-204, the arc closing point 13 of each welding carriage 10 is located in the X-shaped groove between the arc plate 1 and the top cover plate 2. The arc closing point 13 is prone to defects and is set in the X-shaped groove between the arc plate 1 and the top cover plate 2 to facilitate removal before the circumferential seam welding.

[0096] In the above step 202, the second preset distance L2 is two-thirds of the depth of the outer portion 8 of the X-shaped groove.

[0097] The first preset distance L1 is 0-1 mm, and finally all the outer parts 8 of the X-shaped groove are filled to the first preset distance L1 of the outer wall of the tile, which is to facilitate the problem of welding trolley over-welding when welding the annular X-shaped groove formed between the arc plate 1 and the top cover plate 2. Fig.10 and Fig.11As shown, when welding the annular X-shaped groove formed between the arc plate 1 and the top cover plate 2, a magnetic trolley track 11 will be laid. The magnetic trolley track 11 can be directly magnetically attracted to the spherical head. When passing through the X-shaped groove between two adjacent arc plates 1, the groove depth is greatly reduced because the first preset distance L1 has been filled. At this time, a stainless steel plate 14 can be laid at the groove first, and then the magnetic trolley track 11 can be laid, so that the welding trolley 10 can pass through the weld stably and unaffected. The stainless steel plate 14 can be fixed on the groove with a heat-resistant tape. The stainless steel plate 14 is non-magnetic and can prevent the welding trolley 10 from being adsorbed to the bottom of the vehicle.

[0098] The magnetic trolley track 11 can be made of rubber flexible material to fit the linear shape of the spherical head.

[0099] Among them, see Fig.12 As shown, Fig.12 The middle arrow indicates the moving direction of the welding carriage 10. In step 104, the outer portion 8 of the X-shaped groove between the adjacent top cover plates 2 is welded to fill it to a first preset distance L1 below the outer wall surface of the tile, which specifically includes the following steps:

[0100] 301: Along the extension direction of the X-shaped groove, a welding carriage 10 is arranged at both ends of the top cover plate 2.

[0101] 302: driving two welding carriages 10 to move towards each other and perform welding to fill the space to a first preset distance L1 below the outer wall of the tile, and the arc starting times of the two welding carriages 10 are separated by a preset time.

[0102] Two welding carriages 10 are used for staggered welding from bottom to top. The arc starting is staggered by a preset time during welding. The specific duration can be controlled according to actual needs. For example, the staggered time satisfies the moving distance difference of the two welding carriages 10 by 300mm. Staggered welding can facilitate the grinding of the arc crater.

[0103] In step 302 , the arc starting point of each welding carriage 10 is located in the X-shaped groove between the arc plate 1 and the top cover plate 2 .

[0104] Among them, see Fig.13 As shown, Fig.13 The middle arrow indicates the moving direction of the welding carriage 10. In step 104, the outer portion 8 of the X-shaped groove between the arc plate 1 and the top cover plate 2 is welded to fill it to a first preset distance L1 below the outer wall of the tile, which specifically includes the following steps:

[0105] 401: Arrange multiple welding carriages 10 at equal distances along the circumference of the magnetic carriage track 11.

[0106] For example, as an example, Fig.13There are three welding carriages 10 arranged in the middle, and the three welding carriages 10 are evenly distributed according to a central angle of 120°.

[0107] 402: Drive each welding trolley 10 to move synchronously and in the same direction along the circumference of the magnetic trolley track 11, and perform welding to fill to a first preset distance L1 below the outer wall surface of the tile.

[0108] When welding, the two can be moved synchronously and in the same direction in a clockwise direction or in a counterclockwise direction.

[0109] In step 402, the arc starting point and arc ending point 13 of each welding carriage 10 are staggered from the T-joint 6, and the T-joint 6 is formed at the intersection of the X-shaped grooves between the adjacent arc plates 1 and the X-shaped grooves between the arc plates 1 and the top cover plate 2. The staggered distance can be determined according to actual needs. For example, as an example, it is staggered by 200 mm.

[0110] When welding the X-shaped grooves between adjacent arc plates 1, the arc ending point 13 is located in the X-shaped groove between the arc plate 1 and the top cover plate 2, and when welding the X-shaped grooves between adjacent top cover plates 2, the arc starting point is located in the X-shaped groove between the arc plate 1 and the top cover plate 2. Therefore, before performing step 402, it is necessary to perform root cleaning at the position of the T-joint 6, specifically by removing, grinding and trimming through air planing.

[0111] See also Fig.14 and Fig.15 As shown, in step 105, after the outer portion 8 of the X-shaped groove is filled, the tire frame connection is cut off, the spherical head is turned over so that the opening is placed on the tire frame facing upward, and the root cleaning is performed, and the inner portion 7 of the X-shaped groove is cleaned, which specifically includes the following steps:

[0112] 501: According to the order of cleaning the X-shaped grooves between the adjacent arc plates 1, between the adjacent top cover plates 2, and then between the arc plates 1 and the top cover plates 2, first use manual carbon arc air planer to clean the roots so that the depth of the inner part 7 of each X-shaped groove is consistent, and then use a plasma root cleaning trolley in conjunction with a magnetic trolley track 11 to correct and straighten the inner part 7 of the X-shaped groove, with a groove width of 42-44mm and a depth of 30-32mm.

[0113] Because root cleaning will reduce the effective thickness of the weld and reduce its strength, the purpose of adopting the above-mentioned root cleaning sequence is to prevent welding deformation due to the rigidity of the head after the weld is completely cleaned.

[0114] 502: Finally, polish it clean to reveal the metallic luster of the carbide layer.

[0115] In the above step 106 , the welding of the inner portion 7 of the X-shaped groove is performed in the same manner as the welding of the outer portion 8 of the X-shaped groove in step 104 .

[0116] Specifically, welding the inner portion 7 of the X-shaped groove includes the following steps:

[0117] Combination Fig.16 , Fig.17 , Fig.18 , Fig.19 , Fig. 20 As shown, a multi-layer and multi-pass welding method is adopted, and a welding trolley 10 is used to weld the inner part 7 of the X-shaped groove between adjacent curved plates 1 to fill it to a distance lower than the first preset distance L1 of the inner wall of the tile, and the inner part 7 of the X-shaped groove between adjacent top cover plates 2 is welded to fill it to a distance lower than the first preset distance L1 of the inner wall of the tile; the magnetic trolley track 11 is arranged in a circle to cover all the curved plates 1, and a multi-layer and multi-pass welding method is adopted, and a welding trolley 10 is used to weld the inner part 7 of the X-shaped groove between the curved plate 1 and the top cover plate 2 to fill it to a distance lower than the first preset distance L1 of the inner wall of the tile.

[0118] Among them, see Fig.16 and Fig.17 As shown, Fig.16 The middle arrow indicates the moving direction of the welding carriage 10. The inner part 7 of the X-shaped groove between the adjacent top cover plates 2 is first welded to fill it to a first preset distance L1 below the inner wall surface of the tile, specifically including:

[0119] 601: Two welding carriages 10 are arranged in the middle of the top cover plate 2 along the extension direction of the X-shaped groove.

[0120] 602: driving the two welding carriages 10 to move in opposite directions and perform welding to fill the space to a first preset distance L1 below the inner wall of the tile, and the arc starting times of the two welding carriages 10 are separated by a preset time.

[0121] Two welding carriages 10 are used for staggered welding from bottom to top. The arc starting is staggered by a preset time during welding. The specific duration can be controlled according to actual needs. For example, the staggered time satisfies that the moving distance of the two welding carriages 10 differs by 300mm. Staggered welding can facilitate the grinding of the arc crater.

[0122] In step 602 , the arc closing point of each welding carriage 10 is located in the X-shaped groove between the arc plate 1 and the top cover plate 2 .

[0123] Among them, see Fig.18 and Fig.19As shown, the inner part 7 of the X-shaped groove between the adjacent arc-shaped plates 1 is welded to fill it to a first preset distance L1 below the inner wall surface of the tile, specifically including:

[0124] 701: Arrange the X-shaped grooves between the adjacent arc-shaped plates 1 in sequence and divide them into two sequence groups, namely an odd-numbered sequence group and an even-numbered sequence group.

[0125] for example, Fig.18 There are ten curved plates 1, which are divided into two serial groups, each with five. The odd serial group includes the curved plates 1 with serial numbers of one, three, five, seven and nine, and the even serial group includes the curved plates 1 with serial numbers of two, four, six, eight and ten.

[0126] 702: See Fig.18 , Fig.19 As shown, Fig.18 and Fig.19 The middle arrow indicates the moving direction of the welding carriage 10. The welding carriage 10 is driven to move from bottom to top along the extension direction of the X-shaped groove, and the inner part 7 of each X-shaped groove in one of the sequence groups is welded synchronously to fill it to a second preset distance L2 below the inner wall surface of the tile.

[0127] Since the opening of the spherical head faces upward, when welding is performed, the direction from bottom to top is from the top cover plate 2 of the spherical head toward the opening side.

[0128] The welding carriage 10 in step 702 moves synchronously to weld the X-shaped groove of one sequence group at a time, and first fills it to the second preset distance L2, in order to prevent excessive welding deformation and insufficient overall strength of the spherical wall from causing desoldering and uneven deformation problems when welding another sequence group.

[0129] 703: See Fig.18 and Fig.19 As shown, the welding carriage 10 is driven to move from bottom to top along the extension direction of the X-shaped groove, and then the inner part 7 of each X-shaped groove in another sequence group is welded synchronously to fill it to a first preset distance L1 below the inner wall surface of the tile, L1<L2.

[0130] 704: Continue to fill the X-shaped groove of the previous sequence group to reduce the second preset distance L2 to the first preset distance L1.

[0131] In the above steps 702-704, the arc starting point of each welding carriage 10 is located in the X-shaped groove between the arc plate 1 and the top cover plate 2. The arc starting point is prone to defects and is set in the X-shaped groove between the arc plate 1 and the top cover plate 2 to facilitate removal before circumferential seam welding.

[0132] In the above step 702, the second preset distance L2 is two-thirds of the depth of the inner portion 7 of the X-shaped groove.

[0133] The first preset distance L1 is 0-1mm, and eventually all the inner parts 7 of the X-shaped grooves are filled to the first preset distance L1 of the inner wall of the tile. The purpose is to facilitate the problem of over-welding of the welding trolley when welding the annular X-shaped groove formed between the arc plate 1 and the top cover plate 2.

[0134] See also Fig. 20 As shown, after the outer side and the inner side of the spherical head are welded and filled, the above step 107 is started to weld the cover layer 12.

[0135] The capping surface adopts 5-pass annealing capping surface, and the capping surface width is required to be 47-52mm. In order to obtain a full and uniform capping surface weld, the width of a single capping surface weld should be controlled at 18mm. The capping surface welding sequence is: first weld the inside of the spherical head and then turn over and weld the outside of the spherical head, first weld the X-shaped groove between adjacent arc plates 1, then weld the X-shaped groove between the top cover plates 2, and finally weld the X-shaped groove between the arc plate 1 and the top cover plate 2.

[0136] When welding the cover of the X-shaped groove between the arc plates 1, due to the influence of the height of the circumferential seam cover layer, manual gas shielded welding is required for 200-250mm at the T-joint. Welding is performed in this cover sequence, and the trolley welding blind area is minimized.

[0137] A multi-layer and multi-pass welding method is adopted, and the arc starting joint areas of each layer and each pass are staggered by a certain distance, such as, as an example, 50 mm.

[0138] Compared with manual arc welding, this application has high welding efficiency, beautiful shape, stable quality, small deformation, and low labor intensity for welders; by using an X-shaped groove with a blunt edge, the bottom is sealed and welded before welding to prevent positioning weld cracking caused by welding deformation.

[0139] The use of trolley rails and other tooling and a reasonable welding sequence can solve the problem of over-welding of T-joints when welding with a welding trolley and reduce welding blind areas.

[0140] The use of manual planing and plasma gouging can ensure that defects are cleaned up and the root straightness and accuracy are guaranteed, which is beneficial to welding.

[0141] In the description of the present application, it should be noted that the terms "upper", "lower", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. Unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be a connection between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present application can be understood according to the specific circumstances.

[0142] It should be noted that, in this application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.

[0143] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A welding method for a large-diameter, large-thickness, high-strength steel spherical head, characterized in that: It includes: Beveling all tiles to form X-shaped bevels with blunt edges, wherein all tiles include a curved plate (1) and a top cover plate (2); On the tire frame, positioning welding is performed on all the tiles; Performing back-welding on the inner side portion (7) of the X-shaped groove to form a back-welding bead (9); The opening of the spherical head is directed downward, and the outer portion (8) of the X-shaped groove is welded, specifically comprising: - using a multi-layer multi-pass welding method, by means of a welding trolley (10), welding the outer portions (8) of the X-shaped grooves between adjacent arc-shaped plates (1) and between adjacent top cover plates (2) to fill the grooves to a first preset distance L1 below the outer wall surface of the tile; - Arrange the magnetic trolley track (11) in a circular shape to cover all the arc-shaped plates (1), and adopt a multi-layer multi-pass welding method to weld the outer portion (8) of the X-shaped groove between the arc-shaped plate (1) and the top cover plate (2) through the welding trolley (10) to fill it to a first preset distance L1 below the outer wall surface of the tile; After cutting with the tire frame, the inner part (7) of the X-shaped groove is cleaned; The opening of the spherical head is facing upward, and the inner part (7) of the X-shaped groove is welded to fill the groove to a first preset distance L1 below the outer wall of the tile; The inner part (7) and the outer part (8) of the X-shaped groove are welded to form a cover layer (12).

2. The welding method of large-diameter, large-thickness, high-strength steel spherical head according to claim 1 is characterized in that: On the tire frame, all the tiles are tack welded, specifically including: Assemble on the tire frame according to the shape of the spherical head; Spot welding each of the tiles to fix them on the tire frame; Along the extension direction of the X-shaped groove between the adjacent arc-shaped plates (1), an arc-starting plate is welded at the end of the X-shaped groove between the adjacent arc-shaped plates (1) to facilitate the movement of the welding carriage (10) when starting an arc; The spot welding comprises: using a mixed gas of rich argon and carbon dioxide as a shielding gas and adopting a solid welding wire in combination with arc welding to perform welding.

3. The welding method of a large-diameter, large-thickness, high-strength steel spherical head according to claim 1, characterized in that: The positioning welding and the backing welding both include preheating before welding and post-heating after welding, the preheating temperature is 120-140°C, and the post-heating temperature is 220-240°C; And / or, the steps for welding the inner part (7) of the X-shaped groove are the same as those for welding the outer part (8) of the X-shaped groove.

4. The welding method of a large-diameter, large-thickness, high-strength steel spherical head according to claim 1 is characterized in that: The outer portion (8) of the X-shaped groove between the adjacent arc-shaped plates (1) is welded to fill the groove to a first preset distance L1 below the outer wall surface of the tile, specifically comprising: Arrange the X-shaped grooves between the adjacent arc-shaped plates (1) in sequence and divide them into two sequence groups, namely an odd-numbered sequence group and an even-numbered sequence group; Along the extension direction of the X-shaped groove, from bottom to top, the welding carriage (10) is driven to move, and the outer portions (8) of each X-shaped groove in one sequence group are welded synchronously to fill the groove to a second preset distance L2 below the outer wall surface of the tile; Along the extension direction of the X-shaped groove, from bottom to top, the welding carriage (10) is driven to move, and then the outer parts (8) of each X-shaped groove in another sequence group are welded synchronously to fill the groove to a first preset distance L1 below the outer wall of the tile, L1 < L2; The filling is continued so that the second preset distance L2 is reduced to the first preset distance L1.

5. The welding method of a large-diameter, large-thickness, high-strength steel spherical head according to claim 4, characterized in that: The second preset distance L2 is two-thirds of the depth of the outer portion (8) of the X-shaped groove; And / or, the first preset distance L1 is 0-1 mm; And / or, the arc closing point (13) of each welding carriage (10) is located in the X-shaped groove between the arc plate (1) and the top cover plate (2).

6. The welding method of large-diameter, large-thickness, high-strength steel spherical head according to claim 1 is characterized in that: The outer portion (8) of the X-shaped groove between the adjacent top cover plates (2) is welded to fill the groove to a first preset distance L1 below the outer wall surface of the tile, specifically comprising: A welding carriage (10) is arranged at both ends of the top cover plate (2) along the extension direction of the X-shaped groove; Driving two welding carriages (10) to move towards each other and perform welding to fill the gap to a first preset distance L1 below the outer wall surface of the tile; The arc starting times of the two welding carriages (10) are separated by a preset time.

7. The welding method of a large-diameter, large-thickness, high-strength steel spherical head according to claim 6, characterized in that: The arc starting point of each welding carriage (10) is located in the X-shaped groove between the arc plate (1) and the top cover plate (2).

8. The welding method of a large-diameter, large-thickness, high-strength steel spherical head according to claim 1 is characterized in that: The outer portion (8) of the X-shaped groove between the arc plate (1) and the top cover plate (2) is welded to fill the outer portion (8) to a first preset distance L1 below the outer wall surface of the tile, specifically comprising: Arranging a plurality of welding carriages (10) at equal distances along the circumference of the magnetic carriage track (11); Each welding carriage (10) is driven to move synchronously and in the same direction, and to perform welding, so as to fill the gap to a first preset distance L1 below the outer wall surface of the tile.

9. The welding method of a large-diameter, large-thickness, high-strength steel spherical head according to claim 8, characterized in that: The arc starting point and arc ending point (13) of each welding carriage (10) are staggered from the T-joint (6), and the intersection of the X-shaped grooves between adjacent arc-shaped plates (1) and the X-shaped grooves between the arc-shaped plates (1) and the top cover plate (2) forms the T-joint (6).

10. The welding method of a large-diameter, large-thickness, high-strength steel spherical head according to claim 1, characterized in that: The inner part (7) of the X-shaped groove is cleaned, specifically comprising: According to the order of cleaning the X-shaped grooves between adjacent arc-shaped plates (1), between adjacent top cover plates (2), and then between the arc-shaped plates (1) and the top cover plates (2), an air planer is first used to clean the grooves so that the inner part (7) of each X-shaped groove has a uniform depth, and then a plasma cleaning trolley is used in conjunction with a magnetic trolley track (11) to correct and straighten the inner part (7) of the X-shaped groove; Finally, polish it clean to reveal the metallic luster of the carbonized layer.

Citation Information

Cited By

  • Machining method for spherical shell seal head of spacecraft fuel tank

    CN119635206A

  • Hastelloy surfacing device and method for gasification furnace cylinder

    CN121131933A