Preparation method of prefabricated T-beam concrete suitable for dry-hot valley region
By optimizing the concrete mix proportion using the full calculation method and Fuller's ideal gradation curve, selecting suitable raw materials and adjusting the proportions, the construction problem of precast T-beam concrete in the hot and dry valley region under high temperature and low humidity conditions was solved, the workability and strength of the concrete were improved, and the construction quality and progress were ensured.
Patent Information
- Application Number
- CN202410760673.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-11-08
AI Technical Summary
When existing concrete mix designs are applied in hot and dry valley regions, the water-cement ratio is too high and the amount of cementitious materials is too low, resulting in poor concrete workability, slow strength and elastic modulus growth, and difficulty in meeting the construction requirements in high temperature and low humidity environments.
By employing a full calculation method combined with Fuller's ideal gradation curve, suitable raw materials were selected, and the concrete mix proportions were optimized through laboratory testing and adjustments. These proportions included the ratios of cementitious materials, coarse and fine aggregates, and admixtures. Mineral powder was added to improve workability and reduce heat of hydration.
It improved the workability and strength of concrete in hot and dry valleys, shortened the production cycle, and ensured construction quality and project progress.
Smart Images

Figure CN118906229A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of prefabricated T-beam concrete mix design in dry and hot river valley areas, and in particular to a preparation method of prefabricated T-beam concrete suitable for dry and hot river valley areas. Background Art
[0002] Dry hot valley refers to a high temperature, low humidity valley area, mostly distributed in tropical or subtropical regions. Precast T-beams are a widely used structural form in highway construction. Their unique structure, coupled with the unique climatic conditions in dry hot valleys, poses challenges to the quality of precast T-beam concrete construction. Concrete mix design, as the primary link in controlling the quality of concrete pouring, plays an important role in controlling the quality of precast T-beam concrete construction.
[0003] The existing concrete mix proportion is mainly based on the concrete strength grade combined with empirical formula to calculate the trial mix strength and water-cement ratio, and then determine the water consumption based on the designed slump of concrete, the type of coarse aggregate and the maximum nominal particle size; calculate the amount of cementitious material; select the sand ratio based on the water-cement ratio, designed slump, the type of coarse aggregate and the maximum nominal particle size; calculate the mass of coarse and fine aggregates per cubic meter of concrete in combination with the proposed concrete trial mix unit mass, and make fine adjustments based on the trial mix situation at a later stage.
[0004] The existing concrete mix design is semi-calculated and combined with experience. The calculated concrete mix has a relatively large water-cement ratio, a relatively small amount of cementitious materials, relatively poor concrete working performance, and slow growth of concrete strength and elastic modulus. It is not conducive to the production of prefabricated T-beams in river valleys with high temperature and low humidity and high template turnover requirements. How to carry out mix design scientifically, reasonably and objectively in the experimental design stage is a major problem currently faced. Summary of the invention
[0005] The purpose of the present invention is to propose a preparation method for prefabricated T-beam concrete suitable for dry and hot river valley areas in order to maintain the stability of concrete in dry and hot river valley areas, master the technology of improving the working performance of concrete, and enhance the strength and elastic modulus of concrete.
[0006] In order to achieve the above object, the present invention adopts the following technology: a preparation method of prefabricated T-beam concrete suitable for dry hot valley areas, comprising the following steps:
[0007] S1. Comprehensively consider the economy, material applicability and material reserves, select appropriate raw materials and prepare for the subsequent concrete mix;
[0008] S2. Combine the preliminarily selected raw materials and conduct relevant tests to verify whether the material properties meet the specifications and design requirements;
[0009] S3. Based on the test results of the primary raw materials and the ground material conditions, determine the raw materials for the concrete mix ratio on the basis of considering economy, applicability and quantity;
[0010] S4. Refer to the design and relevant specifications of the project, and calculate the concrete test strength, water-cement ratio, water dosage, cementitious material dosage, and coarse and fine aggregate dosage in turn according to the design strength;
[0011] S5. In order to improve the workability of the concrete mixture and reduce the hydration heat of the concrete mixture, add an appropriate amount of mineral powder to the mix material;
[0012] S6. The current mix ratio only considers the maximum aggregate size, and its dosage does not consider the aggregate gradation; based on the calculation of the full calculation method, the particle gradation analysis is carried out according to the formula of Fuller's ideal gradation curve;
[0013] S7. Conducting laboratory tests on various data related to the performance of the trial-mixed concrete mixture and the performance of the hardened concrete to determine the performance of the concrete mixture and the hardened concrete;
[0014] S8. Prepare the concrete mix according to the construction proportion and make adjustments based on the actual performance of the concrete;
[0015] S9. Determine the concrete mix ratio.
[0016] As a further description of the above technology, a method for preparing prefabricated T-beam concrete suitable for dry hot valley areas is as follows:
[0017] S1 takes comprehensive consideration from the perspectives of economy, material applicability, and material reserves. The raw materials include cementitious materials (cement, mineral powder), coarse and fine aggregates, and admixtures (water reducers).
[0018] As a further description of the above technology, a method for preparing prefabricated T-beam concrete suitable for dry hot valley areas is as follows:
[0019] The preliminarily selected raw materials are inspected, and appropriate inspection methods and standards are used to conduct random inspections on the content of various substances in each raw material, as well as information such as material strength, to ensure that the materials meet the experimental standards and reduce the errors in the experimental results.
[0020] As a further description of the above technology, a method for preparing prefabricated T-beam concrete suitable for dry hot valley areas is as follows:
[0021] In S4, on the basis of relevant specifications such as JGJ 55-2011, the mix design is carried out through the full calculation method, which improves the rationality of the proportion of each material by calculation.
[0022] As a further description of the above technology, a method for preparing prefabricated T-beam concrete suitable for dry hot valley areas is as follows:
[0023] In order to improve the workability of concrete mixture and reduce the hydration heat of concrete mixture, S75 grade mineral powder is used in S5; referring to the relevant requirements of JGJ55-2011 specification, a 10% addition amount is adopted without affecting the amount of each material in the existing mix ratio.
[0024] As a further description of the above technology, a method for preparing prefabricated T-beam concrete suitable for dry hot valley areas is as follows:
[0025] In S6, Fuller's ideal gradation curve is used to carry out targeted blending according to the gradation of ground material aggregates, and the density of concrete is further improved through the application of Fuller's ideal gradation curve.
[0026] As a further description of the above technology, a method for preparing prefabricated T-beam concrete suitable for dry hot valley areas is as follows:
[0027] The performance of concrete mixture and hardened concrete is tested and adjusted in the laboratory, and the construction concrete mix ratio is configured and adjusted according to the mix ratio that meets the test requirements, and the concrete mix ratio is finally determined.
[0028] In summary, due to the use of the above-mentioned technology, a method for preparing prefabricated T-beam concrete suitable for dry and hot valley areas has the following beneficial effects:
[0029] The existing concrete mix design is semi-calculated and combined with experience. The calculated concrete mix has a relatively large water-binder ratio and a relatively small amount of cementitious materials, so the concrete workability is relatively poor, and the concrete strength and elastic modulus increase slowly. Combined with the ground material and climate conditions, the concrete mix "full calculation method" and "Fuller's ideal gradation curve" are used to quickly obtain the concrete mix suitable for precast T-beams in dry and hot valley areas, so as to avoid the situation where the existing concrete mix design under high temperature and low humidity climate conditions results in poor concrete workability and slow growth of concrete strength and elastic modulus. This has greatly improved the quality of the precast T-beam concrete of the project, shortened the production cycle, ensured the smooth acceptance of the project, and achieved significant social and economic effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The flowchart corresponding to the steps of preparing prefabricated T-beam concrete in the dry-hot valley region according to the present invention is shown; Figure 2 The aggregate gradation curve corresponding to the preparation steps of prefabricated T-beam concrete in the dry hot valley area according to the present invention is shown. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technology in the embodiments of the present invention, a method for preparing prefabricated T-beam concrete suitable for dry and hot valley areas. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] like Figure 1-2 As shown, the present invention provides a method for preparing prefabricated T-beam concrete suitable for dry-hot river valley areas, comprising the following steps:
[0033] S1. Comprehensively consider the economy, material applicability and material reserves, select appropriate raw materials and prepare for the subsequent concrete mix;
[0034] S2. Combine the preliminarily selected raw materials and conduct relevant tests to verify whether the material properties meet the specifications and design requirements;
[0035] S3. Based on the test results of the primary raw materials and the ground material conditions, determine the raw materials for the concrete mix ratio on the basis of considering economy, applicability and quantity;
[0036] S4. Refer to the design and relevant specifications of the project, and calculate the concrete test strength, water-cement ratio, water dosage, cementitious material dosage, and coarse and fine aggregate dosage in turn according to the design strength;
[0037] S5. In order to improve the workability of the concrete mixture and reduce the hydration heat of the concrete mixture, add an appropriate amount of mineral powder to the mix material;
[0038] S6. The current mix ratio only considers the maximum aggregate size, and its dosage does not consider the aggregate gradation; based on the calculation of the full calculation method, the particle gradation analysis is carried out according to the formula of Fuller's ideal gradation curve;
[0039] S7. Conducting laboratory tests on various data related to the performance of the trial-mixed concrete mixture and the performance of the hardened concrete to determine the performance of the concrete mixture and the hardened concrete;
[0040] S8. Prepare the concrete mix according to the construction proportion and make adjustments based on the actual performance of the concrete;
[0041] S9. Determine the concrete mix ratio.
[0042] In further detail, S1 comprehensively considers the economy, material applicability and material reserves. The raw materials involve cementitious materials (cement, ordinary silicate cement is selected, which has fast coagulation and hardening, high early strength and late strength, and is suitable for concrete with early strength requirements, high-strength concrete and prestressed engineering, and has good durability such as carbonization resistance, frost resistance and wear resistance; the cement grade is 52.5 grade (cement dosage, hydration heat, concrete strength guarantee rate in dry hot valley areas), mineral powder, and commonly used mineral admixtures mainly include fly ash, slag powder, natural zeolite powder, silica fume and its composites, which have the advantages of saving cement dosage, reducing costs, and having volcanic ash effect, increasing concrete Soil compression, tension, flexural and shear strength, significantly reduce concrete hydration heat, improve concrete workability, reduce segregation and bleeding, can inhibit alkali-aggregate reaction, significantly reduce concrete bleeding, improve cement concrete workability), coarse and fine aggregate (fine aggregate is river sand, try to choose medium sand, river sand particles are smooth and relatively clean; concrete mixture has good performance; coarse aggregate is crushed stone, continuous grading), admixture (water reducer is polycarboxylic acid high-performance water reducer with low dosage, high water reduction rate, good slump retention, high compressive strength ratio, green environmental protection, high durability, cost saving, excellent working performance, relatively low carbonization, and good finish of the formed appearance).
[0043] As shown in the following table, the preliminarily selected raw materials are inspected, and appropriate inspection methods and inspection standards are used to conduct sampling inspections on the content of various substances in each raw material and the material strength and other information to ensure that the materials meet the experimental standards and reduce the error of the experimental results.
[0044] Raw Materials - Cement Test Table
[0045]
[0046] Raw Materials - Fine Aggregate Test Table
[0047]
[0048] Sand is divided into Class I, Class II and Class III according to technical requirements. Class I is suitable for concrete with a strength grade greater than C60; Class II is suitable for concrete with strength equal to C60 and anti-freeze, anti-seepage or other requirements; Class III is suitable for concrete and masonry mortar with a strength grade less than C30; 2. Natural sand includes river sand, lake sand, mountain sand, desalinated sea sand, and artificial sand includes machine-made sand and mixed sand; 3. Stone powder content refers to the content of particles with a particle size less than 0.075mm; 4. Sand 1 should not be mixed with grass roots, leaves, branches, plastics, coal blocks, slag and other debris; 5. When there is doubt about the firmness of the sand, a firmness test should be conducted; 6. When the alkali-aggregate reaction does not meet the requirements in the table, technical measures to inhibit the alkali-aggregate reaction should be taken; 7. Particle analysis tests should also be carried out;
[0049] Raw Materials - Coarse Aggregate Test Table
[0050]
[0051] 1. Class I is suitable for concrete with strength grade greater than C60; Class II is suitable for concrete with strength grade of C30-C60 and with frost resistance, anti-seepage or other requirements; Class D is suitable for concrete with strength grade less than C30.
[0052] 2. The coarse aggregate should not be mixed with grass roots, leaves, branches, plastics, coal blocks, slag and other debris. 3. In addition to meeting the requirements in the table, the ratio of the compressive strength of the rock to the concrete strength grade should not be less than 1.5. The rock strength should first be provided by the production unit, and the crushing value index can be used for quality control in the project. 4. When the coarse aggregate contains granular total sulfuric acid or sulfide impurities, special inspections should be carried out to confirm that it can meet the durability requirements of concrete before it can be used. 5. When pebbles are crushed into gravel, there should be two or more crushing surfaces, and the crushing surface should be no less than 70%; 7. Particle analysis tests should also be carried out;
[0053] Raw materials-additive (polycarboxylic acid high performance water reducer) test table
[0054]
[0055] 1. When testing the water reduction rate, air content, water seepage rate ratio, compressive strength ratio, setting time difference and shrinkage ratio, the slump of concrete should be 80±10mm.
[0056] 2. The cement used for random inspection and testing should be engineering cement.
[0057] Raw materials - mineral powder test table
[0058]
[0059] In more detail, S4 uses the full calculation method to design the mix ratio based on JGJ 55-2011 and other relevant specifications, and refers to the design and relevant specification requirements of the project, according to the design strength f cu,k =50Mpa, σ is taken as 6.0Mpa, the volume percentage of paste and aggregate is fixed at 35:65, the paste volume Ve is taken as 350, the air volume Va in the paste is taken as 20, and the concrete trial strength, water-binder ratio, water dosage, cementitious material dosage, and coarse and fine aggregate dosage are calculated in turn;
[0060] 1. The concrete trial strength is:
[0061] f cu,0 ≥f cu,k +1.645σ
[0062] Where fcu,0 —Concrete trial mix strength, MPa;
[0063] f cu,k —Standard value of concrete cube compressive strength, MPa; here we take the design strength grade value of concrete, 50MPa;
[0064] σ—Standard deviation of concrete strength, MPa; according to the design strength grade of concrete and f cu,0 ≥f cu,k +1.645σ, take 6.0MPa;
[0065] Standard deviation of concrete strength σ value
[0066]
[0067] The calculated concrete with design strength grade C50 has a trial mix strength of 59.9Mpa;
[0068] 2. Water-cement ratio is
[0069]
[0070] Where W is the amount of water used per cubic meter, kg;
[0071] F—amount of admixture per cubic meter of concrete mixture, kg;
[0072] C—cement consumption per cubic meter of concrete mixture, kg;
[0073] f ce —28d compressive strength of cementitious material mortar, which can be measured, MPa; take 52.5MPa;
[0074] A, B—regression coefficients; the regression coefficients can be adopted from the following table depending on the type of coarse aggregate used;
[0075] Regression coefficient A, B selection table
[0076]
[0077] The calculation is 0.3498;
[0078] 3. Water usage:
[0079]
[0080] Where V e —Slurry volume, generally 350;
[0081] V a —The volume of air in the slurry is generally 20;
[0082] x—volume dosage of mineral admixture in cementitious materials, x=0%;
[0083] p f —Density of mineral admixture, g / cm 3 ;
[0084] p c —Cement density, g / cm 3 ; Experimental result: 3.10
[0085] The calculation is 165kg;
[0086] 4. Amount of cementitious material:
[0087]
[0088] Where m c+f —Amount of cementitious material used per cubic meter of concrete mixture, kg;
[0089] m w,0 —Water consumption per cubic meter of concrete mixture, kg;
[0090] The calculation is 472kg;
[0091] In order to improve the workability of the mixture and reduce the amount of cementitious materials, 5. Sand ratio can be added:
[0092]
[0093] Where S p —Sand rate, %;
[0094] The calculation is 40.8%;
[0095] 6. The amount of coarse and fine aggregate is:
[0096] m s =(100+W)p s
[0097] m g =(1000-V es -V w ) g
[0098] Where m s —Amount of fine aggregate per cubic meter of concrete mixture, kg; calculated to be 710 kg;
[0099] m g —Amount of coarse aggregate per cubic meter of concrete mixture, kg; calculated to be 1043 kg;
[0100] p s —Apparent density of fine aggregate, g / cm 3; Determined by test to be 2.68g / cm 3 ;
[0101] p g —Apparent density of coarse aggregate, g / cm 3 ; Determined by test to be 2.71g / cm 3 ;
[0102] p gd —Bulk density of coarse aggregate, g / cm 3 ; Determined by test to be 1.52g / cm 3 ;
[0103] V es —Dry mortar volume per cubic meter of concrete mixture, cm 3 ; V es =1000(1-p gd / p g ); calculated to be 439cm 3 , adjusted to 450cm after testing 3 ;
[0104] The above calculations show that the total calculation method mix ratio is: m c,0 :m s :m g :m w,0 =478:710:1043:165.
[0105] In order to improve the workability of concrete mixture and reduce the hydration heat of concrete mixture, S75 grade mineral powder is used in S5; referring to the relevant requirements of JGJ55-2011 specification, a 10% addition amount is adopted without affecting the amount of each material in the existing mix ratio.
[0106] In further detail, S6 utilizes Fuller's ideal gradation curve to carry out targeted blending according to the gradation of ground material aggregates, and further improves the density of concrete through the application of Fuller's ideal gradation curve.
[0107] The current mix ratio only considers the maximum aggregate particle size, and its usage does not take into account the aggregate grading; based on the full calculation method, the particle grading analysis is carried out according to the Fuller's ideal grading curve formula, and explanations are given for the maximum aggregate particle sizes of 31.5mm, 26.5mm, 19.0mm, 16.0mm, 9.5mm, 4.75mm, 2.36mm, 1.18mm, 60mm, 0.30mm, 0.15mm, and sieve bottom.
[0108] It is planned to use secondary grade crushed stone and natural sand for the test, which will be explained in conjunction with the following aggregate composition calculation table;
[0109] 1. First, conduct screening tests on crushed stone 1, crushed stone 2 and natural sand respectively to obtain the sieve residues of various particle sizes;
[0110] 2. Then, according to the size of the cumulative screen residue, determine the particle size that plays a major role in the crushed stone. From the table, we can see that the cumulative screen residue of 26.5mm in crushed stone 1 reaches 60.8%, which can be seen to play a major role in the coarse particles; the cumulative screen residue of 9.5mm sieve hole diameter in crushed stone 2 reaches 68.4%, which plays a major role;
[0111] 3. Combined with the benchmark gradation curve (Fuller's ideal gradation curve) and the cumulative sieve residue (respective) test results of the particle size that plays a major role in the mixture, determine the amount of crushed stone 1 and crushed stone 2 in the mixture; the cumulative sieve residue of the benchmark gradation curve at a pore size of 26.5 mm is 8.3%, and the cumulative sieve residue of crushed stone 1 at a pore size of 26.5 mm is 60.8%. The percentage of crushed stone 1 in the total aggregate is: 8.3÷60.8≈14%. The percentage of each pore size particle of crushed stone 1 in the mixture can be obtained by multiplying the data in row 1 of the table below by 14% The data in the row corresponding to No. 4 in the table; the cumulative screen residue of 9.5mm sieve hole diameter in the crushed stone No. 2 is 68.4%, which plays a major role; the cumulative screen residue of the benchmark gradation curve under the 9.5mm aperture is 45.1%, combined with the amount of 13.9% corresponding to the 9.5mm aperture of the crushed stone No. 1, the percentage of the crushed stone No. 2 in the mixed material is: (45.1-13.9)÷68.4≈46%, that is, the percentage of each aperture particle of the crushed stone No. 2 in the mixed material can be obtained by multiplying the number of data in the row of No. 2 in the table below by 46% to obtain the data in the row corresponding to No. 5 in the table below;
[0112] 4. Determine the amount of sand: Calculate the amount of sand based on the amount of gravel 1 and gravel 2 determined above; the percentage of sand in the total mixture is: 100-14-46=40% (i.e., sand ratio). Multiply the value in row 3 in the table by 40% to obtain the data corresponding to row 6 in the table below the sand amount. The aggregate grading curve is shown in the figure below.
[0113] Aggregate composition calculation table
[0114]
[0115] 5. As Figure 2 As shown, check the mixture gradation; mix crushed stone 1, crushed stone 2 and sand according to the calculated amounts and then screen them, and count the compliance with the benchmark gradation curve (Fuller's ideal curve). If the deviation is large, adjust the test until the requirements are met.
[0118] The laboratory tests and adjusts the concrete mixture performance and hardened concrete performance according to the table below, and configures and adjusts the construction concrete mix ratio according to the mix ratio that meets the test requirements to finally determine the concrete mix ratio.
[0119] Concrete mixture properties, hardened concrete properties test table
[0120]
[0121] Durability and other related tests can be increased or decreased in combination with design and other related requirements;
[0122] To sum up the concrete mix ratio, the sand and gravel yard of a fixed manufacturer has a fixed production process (such as apparent density and sieve size), so the calculation process is also fixed. Under the action of polycarboxylic acid high-performance water-reducing agent (the dosage of polycarboxylic acid water-reducing agent is mixed according to the manufacturer's recommended dosage), the filling and replacement effects of mineral admixtures can improve the workability of the mixture; the compressive strength and elastic modulus of concrete mixed with graded aggregates obtained using Fuller's theory are improved; the elastic modulus can meet the design requirements at a relatively short age (7d), and the compressive strength of concrete reaches the trial mix strength, which is much greater than the design strength, which is beneficial for ensuring the construction period and carrying out subsequent processes in a timely manner.
[0123] Considering the actual situation on site, the concrete density and bulk density are further improved. Combined with the use of high-performance water-reducing agent and the ground material conditions, the mix ratio is adjusted as follows: m c,0 :m s :m g :m w,0 =485:754:1131:160 The sand ratio is 40%, and the gradation of aggregates of various particle sizes is calculated and adjusted according to Fuller's theory.
[0124] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field within the technical scope disclosed by the present invention, according to the technical method of the present invention for preparing prefabricated T-beam concrete suitable for dry and hot valley areas and its inventive concept, can make equivalent replacements or changes, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing prefabricated T-beam concrete suitable for dry and hot valley areas, characterized in that: The following steps are involved: S1. Comprehensively consider the economy, material applicability and material reserves, select appropriate raw materials and prepare for the subsequent concrete mix; S2. Combine the preliminarily selected raw materials and conduct relevant tests to verify whether the material properties meet the specifications and design requirements; S3. Based on the test results of the primary raw materials and the ground material conditions, determine the raw materials for the concrete mix ratio on the basis of considering economy, applicability and quantity; S4. Refer to the design and relevant specifications of the project, and calculate the concrete test strength, water-cement ratio, water dosage, cementitious material dosage, and coarse and fine aggregate dosage in turn according to the design strength; S5. In order to improve the workability of the concrete mixture and reduce the hydration heat of the concrete mixture, add an appropriate amount of mineral powder to the mix material; S6. The current mix proportion only considers the maximum aggregate size, and its dosage does not consider the aggregate gradation; Based on the calculation results of the full calculation method, the particle gradation analysis is carried out according to the formula of Fuller's ideal gradation curve; S7. Conducting laboratory tests on various data related to the performance of the trial-mixed concrete mixture and the performance of the hardened concrete to determine the performance of the concrete mixture and the hardened concrete; S8. Prepare the concrete mix according to the construction proportion and make adjustments based on the actual performance of the concrete; S9. Determine the concrete mix ratio.
2. The method for preparing prefabricated T-beam concrete suitable for dry-hot river valley areas according to claim 1, characterized in that: S1 takes comprehensive consideration from the perspectives of economy, material applicability, and material reserves. The raw materials include cementitious materials (cement, mineral powder), coarse and fine aggregates, and admixtures (water reducers).
3. The method for preparing prefabricated T-beam concrete suitable for dry-hot river valley areas according to claim 2, characterized in that: The preliminarily selected raw materials are inspected, and appropriate inspection methods and standards are used to conduct random inspections on the content of various substances in each raw material, as well as information such as material strength, to ensure that the materials meet the experimental standards and reduce the errors in the experimental results.
4. The method for preparing prefabricated T-beam concrete suitable for dry-hot river valley areas according to claim 1, characterized in that: In S4, on the basis of relevant specifications such as JGJ 55-2011, the mix design is carried out through the full calculation method, which improves the rationality of the proportion of each material by calculation.
5. The method for preparing prefabricated T-beam concrete suitable for dry-hot river valley areas according to claim 1, characterized in that: In S5, S75 grade mineral powder is used to improve the workability of concrete mixture and reduce the hydration heat of concrete mixture; Referring to the relevant requirements of JGJ55-2011 specification, a 10% admixture is adopted without affecting the amount of each material in the existing mix ratio.
6. The method for preparing prefabricated T-beam concrete suitable for dry-hot river valley areas according to claim 1, characterized in that: In S6, Fuller's ideal gradation curve is used to carry out targeted blending according to the gradation of ground material aggregates, and the density of concrete is further improved through the application of Fuller's ideal gradation curve.
7. The method for preparing prefabricated T-beam concrete suitable for dry-hot river valley areas according to claim 1, characterized in that: The performance of concrete mixture and hardened concrete is tested and adjusted in the laboratory, and the construction concrete mix ratio is configured and adjusted according to the mix ratio that meets the test requirements, and the concrete mix ratio is finally determined.