Cutting method and cutting device for silicon carbide crystal ingot
By forming a modified layer through laser light and combining ultrasonic vibration technology, the efficiency and quality problems of the traditional silicon carbide cutting method are solved, and efficient and accurate silicon carbide ingot cutting is achieved, reducing production costs and environmental pollution risks.
Patent Information
- Application Number
- CN202411175119.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional silicon carbide cutting methods have problems such as slow cutting speed, large material loss, high cutting surface roughness and high equipment costs. Laser cutting technology faces challenges in the field of silicon carbide cutting, precise cutting depth control and cutting quality stability.
Combined with laser irradiation and ultrasonic vibration technology, a modified layer is formed inside the silicon carbide ingot through laser light, and ultrasonic vibration is used to promote crack propagation, achieving non-contact, high-precision cutting, reducing material loss and improving cutting efficiency.
It realizes efficient and precise cutting of silicon carbide ingots, reduces production costs, reduces dependence on chemical solvents and high-strength mechanical forces, reduces the risk of environmental pollution, and supports the large-scale industrial production of silicon carbide devices.
Smart Images

Figure CN118906270A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silicon carbide cutting, and in particular to a method and a device for cutting a silicon carbide ingot. Background Art
[0002] In the field of semiconductor materials, silicon carbide (SiC), as an important third-generation wide bandgap semiconductor material, is widely used in power electronics, communications, automobiles, aviation, aerospace, oil extraction, national defense and other fields due to its excellent properties such as large bandgap, high thermal conductivity, large electron saturation drift rate, high critical breakdown electric field and good chemical stability. As the share of silicon carbide devices in the power semiconductor market gradually increases, the demand for high-quality, low-cost silicon carbide wafers is also growing.
[0003] However, the high hardness (Mohs hardness reaches 9.5, second only to diamond) and brittleness of silicon carbide materials pose great challenges to its processing. Although traditional cutting methods, such as diamond wire saw cutting, can achieve the cutting of silicon carbide wafers, there are problems such as slow cutting speed, large material loss, high cutting surface roughness and high equipment cost. For example: the current cutting time of a 6-inch silicon carbide ingot is about 100 to 120 hours, and the cutting time of an 8-inch silicon carbide ingot is about 160 to 165 hours. These problems not only increase the production cost of silicon carbide devices, but also limit their application in large-scale industrial production.
[0004] Laser cutting technology has gradually become a research hotspot in the field of silicon carbide cutting due to its advantages such as non-contact processing, high precision, high efficiency and low loss. Laser cutting technology uses the interaction between laser and material to separate materials by irradiating the surface or inside of the material with a focused laser. However, in the field of silicon carbide cutting, due to the high hardness and brittleness of silicon carbide, the application of laser cutting technology still faces many challenges, such as thermal effect control, precise control of cutting depth and cutting quality stability. Summary of the invention
[0005] The object of the present invention is to provide a method and a cutting device for cutting silicon carbide ingots, which can combine laser irradiation and ultrasonic vibration cutting technology to achieve non-contact, high-precision cutting of silicon carbide crystals, which not only improves the cutting efficiency and quality, but also reduces material loss.
[0006] The purpose of the present invention is achieved by the following technical solutions:
[0007] In one aspect, the present invention provides a method for cutting a silicon carbide ingot, comprising:
[0008] irradiating the upper surface of the first silicon carbide ingot with a laser to form a modified layer inside the first silicon carbide ingot to obtain a second silicon carbide ingot, wherein the modified layer divides the second silicon carbide ingot into an upper part and a lower part;
[0009] Obtaining a load natural frequency of the second silicon carbide ingot;
[0010] adhering the upper surface of the second silicon carbide ingot to an ultrasonic generator;
[0011] The output frequency of the ultrasonic generator is set according to the load natural frequency and the ultrasonic generator is started to separate the upper part and the lower part of the second silicon carbide ingot to obtain a silicon carbide wafer.
[0012] Further, the step of starting the ultrasonic generator to separate the upper portion and the lower portion of the second silicon carbide ingot to obtain the silicon carbide wafer comprises:
[0013] Starting the ultrasonic generator so that the ultrasonic wave generated by the ultrasonic generator resonates with the upper portion of the second silicon carbide ingot;
[0014] After the ultrasonic wave resonates with the upper part of the second silicon carbide crystal ingot for a set time, the upper part and the lower part of the second silicon carbide crystal ingot are separated to obtain a rough silicon carbide wafer and a third silicon carbide crystal ingot, wherein the lower surface of the rough silicon carbide wafer is a first damaged layer;
[0015] The rough silicon carbide wafer is processed to obtain the silicon carbide wafer.
[0016] Further, the rough silicon carbide wafer is processed to obtain the silicon carbide wafer, comprising:
[0017] Using a first grinding device to perform a thinning and grinding process on the lower surface of the rough silicon carbide wafer to remove the first damaged layer, thereby obtaining the silicon carbide wafer;
[0018] Wherein, the grinding amount of the rough silicon carbide wafer is 30-70 μm.
[0019] Furthermore, the cutting method further comprises:
[0020] Using a second grinding device to perform a thinning and grinding process on the upper surface of the third silicon carbide crystal ingot to obtain a fourth silicon carbide crystal ingot;
[0021] Using a third grinding device to perform a thinning and grinding process on the upper surface of the fourth silicon carbide ingot to obtain a silicon carbide ingot to be cut;
[0022] Wherein, the upper surface of the third silicon carbide ingot is a second damaged layer, and the thickness of the second damaged layer is 20-50 μm.
[0023] Further, the mesh number of the second grinding device is smaller than the mesh number of the third grinding device;
[0024] Furthermore, the grinding amount of the third silicon carbide ingot is 30-60 μm, and the surface finish of the fourth silicon carbide ingot is 12-15 nm;
[0025] Furthermore, the grinding amount of the fourth silicon carbide ingot is 10-30 μm, and the surface finish of the silicon carbide ingot to be cut is 2-5 nm;
[0026] Furthermore, the setting time is 1 to 2 seconds;
[0027] Further, the output frequency of the ultrasonic generator is 90%*load natural frequency to 110%*load natural frequency; and / or,
[0028] The amplitude of the ultrasonic wave is 3 to 10 μm;
[0029] Furthermore, the output power of the ultrasonic generator is 20-500W.
[0030] Further, the obtaining of the rough silicon carbide wafer comprises:
[0031] After the upper and lower parts of the second silicon carbide ingot are separated, the ultrasonic generator is turned off, and the ultrasonic vibrator with the rough silicon carbide wafer attached thereto is placed in a water tank;
[0032] Injecting degumming liquid into the water tank so that the degumming liquid submerges the ultrasonic vibrator and the rough silicon carbide wafer;
[0033] The degumming liquid is heated to separate the ultrasonic vibration head from the rough silicon carbide wafer.
[0034] Further, the step of irradiating the upper surface of the first silicon carbide ingot with laser light includes:
[0035] vertically arranging a laser emitter above the first silicon carbide ingot, focusing the laser emitted by the laser emitter on the inside of the first silicon carbide ingot, and controlling the laser emitter to move along a preset path at a preset speed;
[0036] The distance between the position where the laser is focused on the inside of the first silicon carbide ingot and the upper surface of the first silicon carbide ingot is the sum of the thickness of the silicon carbide wafer and the preset grinding amount;
[0037] Further, the preset path includes a parallel path group and / or a vertical path group, the parallel path group includes a plurality of parallel paths arranged at equal intervals, the vertical path group includes a plurality of vertical paths arranged at equal intervals, and the parallel paths and the vertical paths are perpendicular to each other;
[0038] Furthermore, the distance between two adjacent parallel paths is 60 to 350 μm;
[0039] Furthermore, the distance between two adjacent vertical paths is 60 to 350 μm;
[0040] Furthermore, the preset speed is 100-600 mm / s;
[0041] Furthermore, the wavelength of the laser is 355 to 1080 nm;
[0042] Furthermore, the pulse width of the laser is 20ps to 5ns;
[0043] Furthermore, the frequency of the laser irradiation is 30 to 40 KHZ;
[0044] Furthermore, the cross-sectional area of the modified layer is the same as the cross-sectional area of the first silicon carbide ingot.
[0045] Further, the ultrasonic generator includes an ultrasonic vibration head, and the diameter of the ultrasonic vibration head is greater than or equal to the diameter of the first silicon carbide ingot;
[0046] Preferably, the cross-sectional area of the ultrasonic vibrator is 115% to 130% of the cross-sectional area of the first silicon carbide ingot;
[0047] Furthermore, adhering the upper surface of the second silicon carbide crystal ingot to the ultrasonic generator includes: providing an adhesive layer between the upper surface of the second silicon carbide crystal ingot and the ultrasonic vibration head.
[0048] In another aspect, the present invention provides a silicon carbide ingot cutting device, comprising:
[0049] A laser emitter, configured to emit a laser beam to irradiate the upper surface of the first silicon carbide ingot, so as to form a modified layer inside the first silicon carbide ingot, thereby obtaining a second silicon carbide ingot;
[0050] A processing device, used for obtaining the load natural frequency of the second silicon carbide ingot; setting the output frequency of the ultrasonic generator according to the load natural frequency, and generating a start signal;
[0051] An ultrasonic generator is connected to the processing equipment and is used to generate ultrasonic waves after the upper surface of the second silicon carbide ingot adheres to the ultrasonic generator and receives the start signal, so as to separate the upper and lower parts of the second silicon carbide ingot to obtain a silicon carbide wafer.
[0052] Furthermore, the ultrasonic generator includes: a generator body and an ultrasonic vibration head, wherein the generator body is used to generate ultrasonic waves; the ultrasonic vibration head is arranged at the output end of the generator body, and is used to transmit the vibration energy of the ultrasonic wave to the second silicon carbide ingot to obtain a rough silicon carbide wafer and a third silicon carbide ingot;
[0053] The silicon carbide ingot cutting device further includes a receiving platform, which is disposed directly below the ultrasonic vibration head and is used to receive the third silicon carbide ingot that falls off from the ultrasonic vibration head.
[0054] Compared with the prior art, the beneficial effects of the present invention include at least:
[0055] The present invention combines laser irradiation and ultrasonic vibration cutting technology, realizes non-contact precise processing through laser, forms a modified layer inside the silicon carbide ingot, and uses the modified layer induced by laser as a cutting path, which can effectively control the cutting depth and direction, minimize material waste, and improve the utilization rate of raw materials; ultrasonic vibration is then used to promote the expansion of cracks along the modified layer, so as to realize the precise separation of the silicon carbide ingot, which not only overcomes the shortcomings of traditional cutting methods, improves the cutting efficiency and quality of silicon carbide wafers, and reduces production costs, but also reduces dependence on chemical solvents or high-intensity mechanical forces, reduces the risk of environmental pollution, and provides strong support for the large-scale industrial production of silicon carbide devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 It is a schematic diagram of step S1 of the method for cutting a silicon carbide ingot provided by the present invention.
[0057] Figure 2 It is a structural schematic diagram of the preset path provided by the present invention.
[0058] Figure 3 It is another structural schematic diagram of the preset path provided by the present invention.
[0059] Figure 4 It is a schematic diagram of step S3 of the method for cutting a silicon carbide ingot provided by the present invention.
[0060] Figure 5 It is a schematic structural diagram of the separation of the upper and lower parts of the second silicon carbide ingot provided by the present invention.
[0061] Figure 6It is a schematic diagram of obtaining a rough silicon carbide wafer provided by the present invention.
[0062] 1. First silicon carbide ingot; 2. Rough silicon carbide wafer; 3. Third silicon carbide ingot; 4. Laser; 5. Modified layer; 6. Lower surface of rough silicon carbide wafer; 7. Upper surface of third silicon carbide ingot; 8. Ultrasonic generator; 9. Ultrasonic vibrator; 10. Ultrasonic amplitude transformer; 11. Adhesive layer; 12. Receiving platform; 13. Water tank; 14. Vertical path group; 15. Parallel path group; 16. Second silicon carbide ingot; 111. Upper surface of first silicon carbide ingot. DETAILED DESCRIPTION
[0063] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided to make the present invention more comprehensive and complete and to fully convey the concepts of example embodiments to those skilled in the art. The same reference numerals in the figures represent the same or similar structures, and thus their repeated description will be omitted.
[0064] The words expressing positions and directions described in the present invention are all explained with reference to the accompanying drawings as examples, but they can be changed as needed, and all such changes are included in the protection scope of the present invention.
[0065] Compared with the current conventional wire-cut silicon carbide ingot, the present invention introduces a cutting method and a cutting device for silicon carbide ingots that can be cut layer by layer and piece by piece, which are described in detail below.
[0066] Please refer to Figures 1 to 6 The method for cutting a silicon carbide ingot provided by the present invention comprises the following steps:
[0067] Step S1: Reference Figure 1 The upper surface 111 of the first silicon carbide ingot is irradiated with laser 4, so that the laser 4 is focused inside the first silicon carbide ingot 1, and a modified layer 5 is formed inside the first silicon carbide ingot 1, thereby obtaining a second silicon carbide ingot 16.
[0068] The cross-sectional area of the modified layer 5 is the same as that of the first silicon carbide crystal ingot 1 , dividing the second silicon carbide crystal ingot 16 into an upper portion and a lower portion.
[0069] It is worth noting that the principle of laser stealth cutting is to use a laser emitter to generate a high-energy-density laser 4 to irradiate the first silicon carbide ingot 1 and penetrate the surface of the first silicon carbide ingot 1. The laser 4 is focused at a certain depth inside the first silicon carbide ingot 1 and scans back and forth, forming a local high-temperature environment inside the first silicon carbide ingot 1, causing changes in the internal structure of the material (such as local microcracks, dislocations, and partial recrystallization), thereby generating a modified layer 5 inside the first silicon carbide ingot 1. Laser stealth cutting of the first silicon carbide ingot 1 is a non-contact cutting method. Since non-contact cutting does not generate mechanical stress, thermal stress, and material debris, it is very suitable for cutting and slicing the first silicon carbide ingot 1, and can obtain ultra-thin silicon carbide wafers and silicon carbide seed crystals.
[0070] In some embodiments, the wavelength of laser 4 is 355-1080nm (for example, 355nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, 1080nm); the pulse width of laser 4 is 20ps-5ns (for example, 20ps, 50ps, 100ps, 1000ps, 10000ps, 100000ps, 1ns, 2ns, 3ns, 4ns, 5ns); the frequency of laser 4 irradiation is 30-40KHZ (for example, 30KHZ, 31KHZ, 32KHZ, 33KHZ, 34KHZ, 35KHZ, 36KHZ, 37KHZ, 38KHZ, 39KHZ, 40KHZ).
[0071] In some embodiments, the first silicon carbide ingot 1 includes but is not limited to industrial-grade, research-grade and test-grade quality ingots, which may be conductive or semi-insulating silicon carbide ingots. In addition, the crystal form of the first silicon carbide ingot 1 includes but is not limited to 4H-SiC, 6H-SiC or 3C-SiC. Further, the thickness of the first silicon carbide ingot 1 is 15 to 35 mm (e.g., 15 mm, 18 mm, 20 mm, 22 mm, 25 mm, 28 mm, 30 mm, 32 mm, 35 mm), and the diameter of the first silicon carbide ingot 1 is 4 to 12 inches (e.g., 4 inches, 5 inches, 6 inches, 7 inches, 8 inches, 9 inches, 10 inches, 11 inches, 12 inches). Preferably, the diameter of the first silicon carbide ingot 1 is 4 to 8 inches (e.g., 4 inches, 5 inches, 6 inches, 7 inches, 8 inches). When used, the surface of the first silicon carbide crystal ingot 1 is thinned and ground by a 8000#-10000# diamond grinding wheel, so that the surface roughness of the first silicon carbide crystal ingot 1 is less than 5nm.
[0072] In some embodiments, the upper surface 111 of the first silicon carbide ingot is irradiated with the laser 4, and the laser 4 emitted by the laser emitter is perpendicular to the upper surface 111 of the first silicon carbide ingot, and repeatedly moves along a preset path at a preset speed. When applied, the preset speed is 100 to 600 mm / s (e.g., 100 mm / s, 150 mm / s, 200 mm / s, 250 mm / s, 300 mm / s, 350 mm / s, 400 mm / s, 450 mm / s, 500 mm / s, 550 mm / s, 600 mm / s).
[0073] For further reference, Figure 2 and Figure 3 , the preset path can be a parallel path group 15 or a vertical path group 14, or the preset path is a combination of the parallel path group 15 and the vertical path group 14. The parallel path group 15 includes a plurality of parallel paths arranged at equal intervals, and the vertical path group 14 includes a plurality of vertical paths arranged at equal intervals, and the parallel paths and the vertical paths are perpendicular to each other. In practical applications, the spacing between two adjacent parallel paths is 60 to 350 μm (e.g., 60 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm), and the spacing between two adjacent vertical paths is 60 to 350 μm (e.g., 60 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm).
[0074] In some embodiments, the distance between the position where the laser 4 is focused on the inside of the first silicon carbide ingot 1 and the upper surface 111 of the first silicon carbide ingot is the sum of the thickness of the silicon carbide wafer and the preset grinding amount. When applied, the distance between the position where the laser 4 is focused on the inside of the silicon carbide ingot 1 and the upper surface 111 of the first silicon carbide ingot is 350 to 1000 μm (for example, 350 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1000 μm); the thickness of the silicon carbide wafer is 0.1 to 1 mm (for example, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm). In actual application, the preset grinding amount is the total thickness of the upper and lower parts removed by grinding after each cutting. The preset grinding amount of the present invention is 70 to 170 μm (for example, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm).
[0075] Step S2 : obtaining the load natural frequency of the second silicon carbide ingot 16 .
[0076] The natural frequency of the load is 20 to 80 kHz, for example, 20 kHz, 30 kHz, 40 kHz, 50 kHz, 60 kHz, 70 kHz or 80 kHz.
[0077] Step S3 : adhering the upper surface of the second silicon carbide ingot 16 to the ultrasonic generator 8 .
[0078] When used, the upper surface of the second silicon carbide ingot 16 is adhered to the ultrasonic vibration head 9 of the ultrasonic generator 8, referring to Figure 4 .
[0079] In some embodiments, the selected operating frequency range of the ultrasonic generator 8 includes the natural frequency of the load, and the ultrasonic generator 8 has a frequency sweep function.
[0080] In some embodiments, the upper surface of the second silicon carbide ingot 16 is adhered to the ultrasonic vibrator 9 of the ultrasonic generator 8 by applying a two-component adhesive on the upper surface of the second silicon carbide ingot 16 and the ultrasonic vibrator 9, and the upper surface of the second silicon carbide ingot 16 is bonded to the ultrasonic vibrator 9. After the two-component adhesive is cured for 0.5 to 1 hour (for example, 0.5 hours, 0.7 hours, 0.9 hours, 1 hour), an adhesive layer 11 is formed to ensure that the upper surface of the second silicon carbide ingot 16 is bonded to the ultrasonic vibrator 9. The ultrasonic wave in the 20-80KHZ band generated by the ultrasonic generator 8 can be transmitted to the upper part of the second silicon carbide ingot 16 through the adhesive layer 11, and does not need to act on the upper part of the second silicon carbide ingot 16 through a liquid medium. When used, the two-component adhesive has the following characteristics: it can penetrate the ultrasonic wave band of 20 to 80 KHZ, cure quickly and is easy to dissolve; the two-component adhesive can be epoxy AB glue or two-component acrylate glue, and preferably, the two-component adhesive is epoxy AB glue.
[0081] When applied, the size of the cross section of the first silicon carbide ingot 1 is the same as the size of the cross section of the second silicon carbide ingot 16. In actual application, the diameter of the ultrasonic vibrator 9 is greater than or equal to the diameter of the first silicon carbide ingot 1. Specifically, the area of the ultrasonic vibrator 9 is greater than 115%*the area of the upper surface 111 of the first silicon carbide ingot. Preferably, the area of the ultrasonic vibrator 9 is 115% to 130%*the area of the upper surface 111 of the first silicon carbide ingot, which can ensure uniform distribution of ultrasound and avoid cracking of the upper part of the second silicon carbide ingot, and can reasonably control costs.
[0082] Step S4: setting the output frequency of the ultrasonic generator 8 according to the natural frequency of the load and starting the ultrasonic generator 8 to separate the upper and lower parts of the second silicon carbide ingot 16 to obtain a silicon carbide wafer.
[0083] When used, the load natural frequency of the second silicon carbide crystal ingot 16 is obtained by using a processing device, the output frequency of the ultrasonic generator 8 is set according to the load natural frequency, and a start signal is generated. The ultrasonic generator 8 is connected to the processing device. After the upper surface of the second silicon carbide crystal ingot 16 adheres to the ultrasonic generator 8 and receives the start signal, ultrasonic waves are generated to separate the upper and lower parts of the second silicon carbide crystal ingot 16 to obtain a silicon carbide wafer.
[0084] The ultrasonic generator 8 of the present invention comprises a generator body and an ultrasonic vibrator 9. The generator body is used to generate ultrasonic waves, and the ultrasonic vibrator 9 is arranged at the output end of the generator body to transmit the vibration energy of the ultrasonic waves to the second silicon carbide ingot 16 to obtain the rough silicon carbide wafer 2 and the third silicon carbide ingot 3.
[0085] When used, the ultrasonic vibrator 9 can be circular and made of stainless steel, having high thermal conductivity, wear resistance and shape adaptability, and can transmit ultrasonic vibration energy to the upper part of the second silicon carbide ingot 16, so as to achieve physical separation of the upper and lower parts of the second silicon carbide ingot 16, so as to obtain a rough silicon carbide wafer and a third silicon carbide ingot 3. Furthermore, a receiving platform 12 is provided below the ultrasonic vibrator 9, and the ultrasonic vibrator 9 faces the upper surface of the receiving platform 12, and the receiving platform 12 receives the third silicon carbide ingot 3 falling off from the ultrasonic vibrator 9.
[0086] Furthermore, the ultrasonic generator 8 also includes an ultrasonic horn 10 (ie, an ultrasonic energy concentrator), which can amplify the particle displacement or velocity of the mechanical vibration and concentrate the ultrasonic energy on a smaller area (ie, energy concentrating).
[0087] In a specific implementation, step S4 includes: step S41 to step S44.
[0088] Step S41: Determine the output frequency of the ultrasonic generator 8 according to the natural frequency of the load.
[0089] According to the load natural frequency, the frequency is automatically adjusted within the set frequency range using the frequency sweeping function of the ultrasonic generator 8, thereby determining the output frequency of the ultrasonic generator 8 (i.e., the resonant frequency of the ultrasonic wave and the second silicon carbide ingot 16). The output frequency of the ultrasonic generator 8 is 90%*load natural frequency to 110%*load natural frequency.
[0090] Step S42 : starting the ultrasonic generator 8 so that the ultrasonic wave generated by the ultrasonic generator 8 resonates with the upper portion of the second silicon carbide ingot 16 .
[0091] When the ultrasonic wave resonates with the upper part of the second silicon carbide ingot 16, the amplitude of the ultrasonic wave is 3 to 10 μm (for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm), and the output power of the ultrasonic wave is 20 to 500 W (for example, 20 W, 50 W, 100 W, 150 W, 200 W, 250 W, 300 W, 350 W, 400 W, 450 W, 500 W).
[0092] Step S43: Reference Figure 5 After the ultrasonic wave resonates with the upper part of the second silicon carbide ingot 16 for a set time, the upper part and the lower part of the second silicon carbide ingot 16 are separated to obtain a rough silicon carbide wafer 2, and the lower surface 6 of the rough silicon carbide wafer is the first damaged layer.
[0093] The set time is 1 to 2 seconds, for example, 1s, 1.1s, 1.2s, 1.3s, 1.4s, 1.5s, 1.6s, 1.7s, 1.8s, 1.9s or 2s.
[0094] The principle of separating the upper and lower parts of the second silicon carbide crystal ingot 16 is that the upper part of the second silicon carbide crystal ingot 16 generates micro-vibrations of tens of thousands to hundreds of thousands times per second under the action of ultrasonic waves (the specific number is related to the output frequency of the ultrasonic generator 8). Due to the existence of the modified layer 5, the ability of ultrasonic waves to propagate to the lower part of the second silicon carbide crystal ingot 16 is cut off, so that the ultrasonic waves cannot propagate to the lower part of the second silicon carbide crystal ingot 16, and the lower part of the second silicon carbide crystal ingot 16 does not make any micro-vibrations, thereby achieving physical separation of the upper and lower parts of the second silicon carbide crystal ingot 16. The upper portion of the second silicon carbide crystal ingot 16 is adhered to the ultrasonic vibrator 9 by the adhesive layer 11, and the lower portion of the silicon carbide crystal ingot 1 falls onto the supporting platform 12 below under the action of gravity. Since the distance between the lower portion of the second silicon carbide crystal ingot 16 and the supporting platform 12 is short (1 to 100 mm, for example, 1 mm, 5 mm, 10 mm, 20 mm, 30 mm, 40 mm, 50 mm, 60 mm, 70 mm, 80 mm, 90 mm, 100 mm), and the area of the supporting platform 12 is greater than or equal to the area of the cross-section of the second silicon carbide crystal ingot 16 (for example, the diameter of the receiving platform 12 is 12 inches), the lower portion of the second silicon carbide crystal ingot 16 will not break when it falls on the supporting platform 12 below, and can remain intact.
[0095] Further, refer to Figure 6After the upper and lower parts of the second silicon carbide ingot 16 are separated, the power supply of the ultrasonic generator 8 is turned off, and the ultrasonic vibrator 9 with the rough silicon carbide wafer attached is placed in the water tank 13, and a degumming liquid (such as water or a degumming agent, preferably water) is injected into the water tank 13, so that the ultrasonic vibrator 9, the adhesive layer 11, and the rough silicon carbide wafer are all immersed in the degumming liquid. Next, the degumming liquid in the water tank 13 is heated by an electric furnace. When the temperature reaches the specific degumming temperature of the adhesive layer 11 itself (such as 85-95°C), it is immersed for 10-15 minutes (such as 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes or 15 minutes) to make the components of the adhesive layer 11 chemically change and lose viscosity, so that the rough silicon carbide wafer is separated from the adhesive layer 11, and the ultrasonic vibrator 9 is separated from the adhesive layer 11, so that the rough silicon carbide wafer and the ultrasonic vibrator 9 are physically separated. When used, the diameter of the rough silicon carbide wafer is 4 to 8 inches (for example, 4 inches, 5 inches, 6 inches, 7 inches, 8 inches), and the thickness of the rough silicon carbide wafer is 350 to 1000 μm (for example, 350 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm). The thickness of the wafer depends on the depth of the focused scanning of the laser 4 inside the first silicon carbide ingot 1.
[0096] Step S44: Processing the rough silicon carbide wafer to obtain a silicon carbide wafer.
[0097] The first grinding device may be used to perform a thinning and grinding process on the lower surface 6 of the rough silicon carbide wafer to remove the first damaged layer and obtain a silicon carbide wafer.
[0098] When used, the rough silicon carbide wafer is inspected and enters the normal processing procedure after passing the inspection, such as using a diamond grinding wheel to thin and remove the first damaged layer of the lower surface 6 of the silicon carbide wafer. The thickness of the first damaged layer of the rough silicon carbide wafer is 20 to 50 μm (for example, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm). The thickness removed by grinding is 30 to 70 μm (for example, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm). After improving the flatness, it enters the polishing production stage to form a qualified silicon carbide substrate product, that is, a silicon carbide wafer.
[0099] In actual application, after the upper and lower parts of the second silicon carbide ingot 16 are separated, a third silicon carbide ingot 3 can be obtained, and the upper surface 7 of the third silicon carbide ingot is a second damaged layer, and the thickness of the second damaged layer of the third silicon carbide ingot 3 is 20 to 50 μm (for example, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm). In order to be able to perform the next cutting, the cutting method of the present invention also includes: step 5.
[0100] Step 5: Perform a thinning and grinding process on the third silicon carbide ingot 3 to obtain a silicon carbide ingot to be cut.
[0101] Specifically, step S5 includes: step S51 and step S52.
[0102] Step S51: using a second grinding device to perform a thinning and grinding process on the upper surface 7 of the third silicon carbide crystal ingot to obtain a fourth silicon carbide crystal ingot.
[0103] The upper surface 7 of the third silicon carbide crystal ingot is a second damaged layer, and the thickness of the second damaged layer is 20-50 μm.
[0104] During application, a 2000#~3000# diamond grinding wheel is used to thin and grind the upper surface 7 of the third silicon carbide ingot to remove the second damaged layer caused by the laser 4 scanning. The first grinding process removes a thickness of 30 to 60 μm (for example, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm), so that the surface roughness Ra of the upper surface 7 of the third silicon carbide ingot is 12 to 15 nm (for example, 12 nm, 12.5 nm, 13 nm, 13.5 nm, 14 nm, 14.5 nm, 15 nm).
[0105] Step S52: using a third grinding device to perform a thinning and grinding process on the upper surface of the fourth silicon carbide ingot to obtain a silicon carbide ingot to be cut.
[0106] The mesh number of the second grinding device is smaller than the mesh number of the third grinding device.
[0107] During application, a 8000#-10000# diamond grinding wheel is used to precisely thin and grind the upper surface of the fourth silicon carbide ingot, and the second grinding thickness is 10 to 30 μm (for example, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm), so that the smoothness of the upper surface of the silicon carbide ingot to be cut is better improved, and the smoothness Ra of the upper surface of the silicon carbide ingot to be cut is 2 to 5 nm (for example, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm).
[0108] After the above two thinnings, the surface of the silicon carbide ingot to be cut is a mirror surface, and the silicon carbide ingot to be cut is used as a new first silicon carbide ingot 1. At this time, the new first silicon carbide ingot 1 can be used to repeat the above steps S1 to S4 to start producing a second silicon carbide wafer, and the cycle is repeated until the entire first silicon carbide ingot 1 is completely peeled off into silicon carbide wafers, thereby achieving high-efficiency and low-cost cutting of the first silicon carbide ingot 1.
[0109] It should be noted that the present invention can cut silicon carbide wafers of different thicknesses on the same first silicon carbide ingot 1, and the thickness of each silicon carbide wafer can be adjusted and controlled individually to meet the cutting of silicon carbide wafers with different quality requirements, such as the cutting of seed crystals with the highest quality requirements. Generally, the thickness of the seed crystals used for crystal growth is higher than the thickness of the substrate wafer. High-quality silicon carbide seed crystals that meet quality and size requirements can be selectively processed in the first silicon carbide ingot 1. Furthermore, high-quality silicon carbide seed crystals with the best quality and adjustable thickness are cut out from the first silicon carbide ingot 1 and used as seeds for crystal growth. The quality of each part of the first silicon carbide ingot 1 is different. Generally, the crystal quality is the highest in the middle part of the ingot. Due to the special requirements of the seed crystal thickness, traditional wire cutting cannot cut out suitable silicon carbide seed crystals, or in order to obtain suitable seed crystals, it will cause serious waste of materials of the first silicon carbide ingot 1.
[0110] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0111] Example 1-1
[0112] Step S21: Use a high-energy pulse laser with a wavelength of 1064nm, a pulse width of 5ns, a frequency of 30KHZ, a power of 20W, and a spot diameter of 30μm to stealth cut the first silicon carbide ingot 1 with a diameter of 100mm and a thickness of 15mm, focus it at a position with a depth of 350μm in the first silicon carbide ingot 1, and perform unidirectional parallel scanning there to produce a modified layer 5, thereby obtaining a second silicon carbide ingot 16.
[0113] The scanning rate of the laser (ie, the preset speed) is 600 mm / s, and the scanning spacing of the laser (ie, the spacing between parallel paths) is 120 μm.
[0114] Step S22: Bond the second silicon carbide ingot 16 to the ultrasonic vibrator 9 of the ultrasonic generator 8 with a two-component adhesive. After the two-component adhesive is cured for 1 hour, invert the ultrasonic vibrator 9 so that the second silicon carbide ingot 16 is at the bottom and the ultrasonic vibrator 9 is at the top.
[0115] The cross-sectional area of the ultrasonic oscillator 9 is 1.2 times the cross-sectional area of the first silicon carbide crystal ingot 1, and the ultrasonic oscillator 9 can cover the upper surface of the second silicon carbide crystal ingot 16; the operating frequency range of the ultrasonic generator 8 is 20-80KHZ.
[0116] Step S23: measuring the load natural frequency of the second silicon carbide ingot 16, and obtaining that the load natural frequency is 18.90 KHZ.
[0117] Step 24: Turn on the ultrasonic generator 8 with an output frequency of 20 KHz, an ultrasonic amplitude of 3 μm, and an output power of 20 W; when the ultrasonic wave resonates with the upper part of the second silicon carbide crystal ingot 16 for 2 seconds, the silicon carbide wafer and the third silicon carbide crystal ingot 3 are physically separated.
[0118] The silicon carbide wafer is adhered to the ultrasonic vibrator 9 due to the two-component adhesive, and the third silicon carbide ingot 3 falls on the supporting platform 12 below under the action of its own gravity field; the distance between the lower part of the second silicon carbide ingot 16 and the supporting platform 12 is 2 mm.
[0119] Step S25: turn off the ultrasonic generator 8, place the ultrasonic vibrator 9 with the silicon carbide wafer in the water tank 13, inject water 14, so that the ultrasonic vibrator 9, the adhesive layer 11 and the silicon carbide wafer are all immersed in the water; heat the water tank 13 with an electric furnace, and when the water temperature reaches 90 degrees, keep it for 10 minutes to obtain a silicon carbide wafer with a diameter of 100 mm and a thickness of 350 μm.
[0120] Step S26: using a 2000# diamond grinding wheel to grind the third silicon carbide crystal ingot 3 to remove the second damaged layer 7 with a thickness of 40 μm, thereby obtaining a fourth silicon carbide crystal ingot.
[0121] The grinding depth of the third silicon carbide crystal ingot 3 is 50 μm, and the surface finish Ra of the fourth silicon carbide crystal ingot is 15 nm.
[0122] Step S27: Use a 8000# diamond grinding wheel to precisely thin and grind the fourth silicon carbide ingot to obtain a silicon carbide ingot to be cut.
[0123] The grinding amount of the fourth silicon carbide ingot is 10 μm, and the surface finish Ra of the silicon carbide ingot to be cut is 5 nm, and the surface finish is better improved.
[0124] Step S28: taking the silicon carbide ingot to be cut as the first silicon carbide ingot 1, and returning to execute step S21 until the cutting is completed.
[0125] After all the first silicon carbide ingots 1 with a diameter of 4 inches and a thickness of 15 mm are cut, the total number of silicon carbide wafers is 34. Compared with the total number of 23 wafers of the first silicon carbide ingot 1 cut by the conventional multi-wire cutting technology (assuming that the wafer thickness is 350 μm; the wire diameter is 170 μm, and the damage processing thickness is 120 μm), the wafer yield of Example 1 is increased by 56%.
[0126] The output of the film in this embodiment is shown in Table 1.
[0127] Embodiment 1-2:
[0128] Compared with Example 1-1, the main difference between this embodiment and Example 1-2 is that the amplitude of the ultrasonic wave is 4 μm. The output of the film in this embodiment is shown in Table 1.
[0129] Embodiment 1-3:
[0130] Compared with Example 1-1, the main difference between Example 1-3 and this Example is that the amplitude of the ultrasonic wave is 5 μm. The output of this Example is shown in Table 1.
[0131] Embodiment 1-4:
[0132] Compared with Example 1-1, the main difference between Example 1-4 and this embodiment is that the amplitude of the ultrasonic wave is 6 μm. The output of this embodiment is shown in Table 1.
[0133] Embodiment 1-5:
[0134] Compared with Example 1-1, the main difference between Example 1-5 and this Example is that the amplitude of the ultrasonic wave is 7 μm. The output of this Example is shown in Table 1.
[0135] Embodiment 1-6:
[0136] Compared with Example 1-1, the main difference between Example 1-6 and this Example is that the amplitude of the ultrasonic wave is 8 μm. The output of this Example is shown in Table 1.
[0137] Embodiment 1-7:
[0138] Compared with Example 1-1, the main difference between Example 1-7 and this Example is that the amplitude of the ultrasonic wave is 9 μm. The output of this Example is shown in Table 1.
[0139] Embodiment 1-8:
[0140] Compared with Example 1-1, the main difference between Example 1-8 and this example is that the amplitude of the ultrasonic wave is 10 μm. The output of this example is shown in Table 1.
[0141] Embodiment 2:
[0142] Step S21: Use a high-energy pulse laser 4 with a wavelength of 1080nm, a pulse width of 1ns, a frequency of 40KHZ, a power of 23W, and a spot diameter of 25μm to stealthily cut the first silicon carbide ingot 1 with a diameter of 200mm and a thickness of 15mm, focus it at a position with a depth of 500μm in the first silicon carbide ingot 1, and perform a unidirectional parallel scan there to produce a modified layer 5, thereby obtaining a second silicon carbide ingot 16.
[0143] The scanning rate of the laser is 300 mm / s, and the scanning pitch of the laser is 180 μm.
[0144] Step S22: Bond the second silicon carbide ingot 16 to the ultrasonic vibrator 9 of the ultrasonic generator 8 with a two-component adhesive. After the two-component adhesive is cured for 1 hour, invert the ultrasonic vibrator 9 so that the second silicon carbide ingot 16 is at the bottom and the ultrasonic vibrator 9 is at the top.
[0145] The cross-sectional area of the ultrasonic oscillator 9 is 1.25 times the cross-sectional area of the first silicon carbide crystal ingot 1, and the ultrasonic oscillator 9 can cover the upper surface of the second silicon carbide crystal ingot 16; the operating frequency range of the ultrasonic generator 8 is 20-80KHZ.
[0146] Step S23: measuring the load natural frequency of the second silicon carbide ingot 16, and obtaining that the load natural frequency is 19.50 KHZ.
[0147] Step 24: Turn on the ultrasonic generator 8 with an output frequency of 20 KHz, an ultrasonic amplitude of 5 μm, and an output power of 30 W; when the ultrasonic wave resonates with the upper part of the second silicon carbide crystal ingot 16 for 1.8 seconds, the rough silicon carbide wafer 2 and the third silicon carbide crystal ingot 3 are physically separated.
[0148] The rough silicon carbide wafer 2 is adhered to the ultrasonic vibrator 9 due to the two-component adhesive, and the third silicon carbide ingot 3 falls onto the supporting platform 12 below under the action of its own gravity field; the distance between the lower part of the second silicon carbide ingot 16 and the supporting platform 12 is 5 mm.
[0149] Step S25: Turn off the ultrasonic generator 8, place the ultrasonic vibrator 9 with the silicon carbide wafer in the water tank 13, inject water 14, so that the ultrasonic vibrator 9, the adhesive layer 11 and the silicon carbide wafer are all immersed in the water; heat the water tank with an electric furnace, and when the water temperature reaches 90 degrees, keep it for 15 minutes to obtain a rough silicon carbide wafer 2 with a diameter of 200 mm and a thickness of 500 μm.
[0150] Step S26: using a 2000# diamond grinding wheel to grind the third silicon carbide crystal ingot 3 to remove the second damaged layer 7 with a thickness of 45 μm, thereby obtaining a fourth silicon carbide crystal ingot.
[0151] The grinding depth of the third silicon carbide crystal ingot 3 is 60 μm, and the surface finish Ra of the fourth silicon carbide crystal ingot is 16 nm.
[0152] Step S27: Use a 8000# diamond grinding wheel to precisely thin and grind the fourth silicon carbide ingot to obtain a silicon carbide ingot to be cut.
[0153] The grinding amount of the fourth silicon carbide ingot is 20 μm, and the surface finish Ra of the silicon carbide ingot to be cut is 5 nm, and the surface finish is better improved.
[0154] Step S28: taking the silicon carbide ingot to be cut as the first silicon carbide ingot 1, and returning to execute step S21 until the cutting is completed.
[0155] After all the first silicon carbide ingots 1 with a diameter of 200 mm and a thickness of 15 mm are cut, the total number of silicon carbide wafers is 24. Compared with the total number of 18 wafers of the first silicon carbide ingot 1 cut by the conventional multi-wire cutting technology (assuming that the wafer thickness is 500 μm; the wire diameter is 170 μm, and the damage processing thickness is 120 μm), the wafer yield of Example 2 is increased by 33%.
[0156] The output of this embodiment is shown in Table 2.
[0157] Embodiment 3:
[0158] Compared with Example 1-1, the main differences of Example 3 are: the wavelength of laser 4 is 1064nm; the pulse width of laser 4 is 20ps; the preset path includes parallel path group 15 and vertical path group 14. The output of this embodiment is detailed in Table 2.
[0159] Embodiment 4:
[0160] Compared with Example 1-1, the main differences of Example 4 are: the wavelength of laser 4 is 355nm; the spot diameter of laser 4 is 10μm; the pulse width of laser 4 is 4ns; the preset path includes parallel path group 15 and vertical path group 14. The output of this embodiment is detailed in Table 2.
[0161] Embodiment 5:
[0162] Compared with Example 1-1, the main differences of Example 5 are as follows: the wavelength of laser 4 is 1080nm; the spot diameter of laser 4 is 25μm, and the pulse width of laser 4 is 1ns; the preset path includes parallel path group 15 and vertical path group 14. The output of this embodiment is detailed in Table 2.
[0163] Embodiment 6:
[0164] Compared with Example 1-1, the main differences of Example 6 are: the wavelength of laser 4 is 532nm; the spot diameter of laser 4 is 30μm; the pulse width of laser 4 is 40ps; the preset path includes parallel path group 15 and vertical path group 14. The output of this embodiment is detailed in Table 2.
[0165] Example 7-1:
[0166] Compared with Example 4, the main differences of Example 7 are: the natural frequency of the load is 38.9 KHz; the output frequency of the ultrasonic generator is 40 KHz. The output of the film of this embodiment is shown in Table 3.
[0167] Example 7-2:
[0168] Compared with Example 7-1, the main difference between Example 7-2 and this Example is that the amplitude of the ultrasonic wave is 4 μm. The output of this Example is shown in Table 3.
[0169] Example 7-3:
[0170] Compared with Example 7-1, the main difference between Example 7-3 and this Example is that the amplitude of the ultrasonic wave is 5 μm. The output of this Example is shown in Table 3.
[0171] Example 7-4:
[0172] Compared with Example 7-1, the main difference between Example 7-4 and Example 7-1 is that the amplitude of the ultrasonic wave is 6 μm. The output of the film in this example is shown in Table 3.
[0173] Example 7-5:
[0174] Compared with Example 7-1, the main difference between Example 7-5 and this example is that the amplitude of the ultrasonic wave is 7 μm.
[0175] The output of this embodiment is shown in Table 3.
[0176] Example 7-6:
[0177] Compared with Example 7-1, the main difference between this embodiment and Example 1-6 is that the amplitude of the ultrasonic wave is 8 μm.
[0178] The output of this embodiment is shown in Table 3.
[0179] Example 7-7:
[0180] Compared with Example 7-1, the main difference between this embodiment and Example 7-7 is that the amplitude of the ultrasonic wave is 9 μm.
[0181] The output of this embodiment is shown in Table 3.
[0182] Embodiment 7-8:
[0183] Compared with Example 7-1, the main difference between this embodiment and Example 7-8 is that the amplitude of the ultrasonic wave is 10 μm.
[0184] The output of this embodiment is shown in Table 3.
[0185] Example 8-1:
[0186] Compared with Example 5, the main differences of Example 8-1 are: the load natural frequency is 60.5KHz;
[0187] The output frequency of the ultrasonic generator 8 is 60 KHz; the amplitude of the ultrasonic wave is 3 μm. The output of the film in this embodiment is shown in Table 4.
[0188] Example 8-2:
[0189] Compared with Example 8-1, the main difference between Example 8-2 and this Example is that the amplitude of the ultrasonic wave is 4 μm. The output of this Example is shown in Table 4.
[0190] Example 8-3:
[0191] Compared with Example 8-1, the main difference between Example 8-3 and Example 8-1 is that the amplitude of the ultrasonic wave is 5 μm. The output of the film in this example is shown in Table 4.
[0192] Example 8-4:
[0193] Compared with Example 8-1, the main difference between Example 8-4 and Example 8-1 is that the amplitude of the ultrasonic wave is 6 μm. The output of the film in this example is shown in Table 4.
[0194] Example 8-5:
[0195] Compared with Example 7-1, the main difference between Example 8-5 and this Example is that the amplitude of the ultrasonic wave is 7 μm. The output of this Example is shown in Table 4.
[0196] Example 8-6:
[0197] Compared with Example 8-1, the main difference between Example 8-6 and this Example is that the amplitude of the ultrasonic wave is 8 μm. The output of this Example is shown in Table 4.
[0198] Example 8-7:
[0199] Compared with Example 8-1, the main difference between Example 8-7 and Example 8-1 is that the amplitude of the ultrasonic wave is 9 μm. The output of the film in this example is shown in Table 4.
[0200] Example 8-8:
[0201] Compared with Example 8-1, the main difference between this example and Example 8-8 is that the amplitude of the ultrasonic wave is 10 μm. The output of this example is shown in Table 4.
[0202] Example 9-1:
[0203] Compared with Example 6, the main differences of Example 9-1 are: the natural frequency of the load is 80.9 KHz; the output frequency of the ultrasonic generator 8 is 80 KHz; and the amplitude of the ultrasonic wave is 3 μm. The output amount of this example is shown in Table 5.
[0204] Example 9-2:
[0205] Compared with Example 9-1, the main difference between Example 9-2 and this Example is that the amplitude of the ultrasonic wave is 4 μm. The output of this Example is shown in Table 5.
[0206] Example 9-3:
[0207] Compared with Example 9-1, the main difference between Example 9-3 and this Example is that the amplitude of the ultrasonic wave is 5 μm. The output of this Example is shown in Table 5.
[0208] Example 9-4:
[0209] Compared with Example 9-1, the main difference between Example 9-4 and this Example is that the amplitude of the ultrasonic wave is 6 μm. The output of this Example is shown in Table 5.
[0210] Example 9-5:
[0211] Compared with Example 9-1, the main difference between Example 9-5 and Example 9-1 is that the amplitude of the ultrasonic wave is 7 μm. The output of the film in this example is shown in Table 5.
[0212] Example 9-6:
[0213] Compared with Example 9-1, the main difference between Example 9-6 and this Example is that the amplitude of the ultrasonic wave is 8 μm. The output of this Example is shown in Table 5.
[0214] Example 9-7:
[0215] Compared with Example 9-1, the main difference between Example 9-7 and Example 9-1 is that the amplitude of the ultrasonic wave is 9 μm. The output of the film in this example is shown in Table 5.
[0216] Example 9-8:
[0217] Compared with Example 9-1, the main difference between Example 9-8 and this Example is that the amplitude of the ultrasonic wave is 10 μm. The output of this Example is shown in Table 5.
[0218] Embodiment 10:
[0219] Compared with Example 2, the main differences of Example 10 are: the wavelength of laser 4 is 355nm; the pulse width of laser 4 is 5ns; the power of the laser is 10W; the frequency of laser irradiation is 35KHz; the preset speed is 100mm / s; the spacing of the vertical path and the spacing of the parallel path are 60μm; the output power of the ultrasonic wave is 200W; the time for the ultrasonic wave to resonate with the upper part of the second silicon carbide ingot is 1.9s; the output of this embodiment is detailed in Table 2.
[0220] Embodiment 11:
[0221] Compared with Example 6, the main differences of Example 11 are: the diameter of the first silicon carbide ingot is 150 mm, and the thickness is 30 mm; the wavelength of laser 4 is 532 nm; the sum of the thickness of the silicon carbide wafer and the preset grinding amount is 300 μm; the spot diameter of the laser is 20 μm; the pulse width of laser 4 is 100 ps; the power of the laser is 15 W; the frequency of laser irradiation is 35 KHz; the preset speed is 300 mm / s; the spacing of the vertical path and the spacing of the parallel path are 350 μm; the load natural frequency is 19 KHz; the amplitude of the ultrasonic wave is 7.5 μm; the output power of the ultrasonic wave is 300 W; the time for the ultrasonic wave to resonate with the upper part of the second silicon carbide ingot is 2.1 s; the distance between the lower part of the second silicon carbide ingot and the supporting platform is 5 mm; the output amount of this embodiment is detailed in Table 2.
[0222] Embodiment 12:
[0223] Compared with Example 2, the main differences of Example 12 are: the diameter of the first silicon carbide ingot is 150 mm, and the thickness is 35 mm; the wavelength of laser 4 is 1064 nm; the sum of the thickness of the silicon carbide wafer and the preset grinding amount is 400 μm; the spot diameter of the laser is 25 μm; the pulse width of laser 4 is 500 ps; the power of the laser is 20 W; the frequency of laser irradiation is 35 KHz; the preset speed is 400 mm / s; the spacing of the vertical path and the spacing of the parallel path are 200 μm; the load natural frequency is 19 KHz; the amplitude of the ultrasonic wave is 8 μm; the output power of the ultrasonic wave is 400 W; the time for the ultrasonic wave to resonate with the upper part of the second silicon carbide ingot is 2 s; the output of this embodiment is detailed in Table 2.
[0224] Comparative Example 1:
[0225] Compared with Example 1-1, the main difference of Comparative Example 1 is that the spacing between the vertical paths and the spacing between the parallel paths is 400 μm.
[0226] The scanning interval of the laser 4 is too large, which is beyond the applicable range of the present invention, resulting in the inability to peel off the upper and lower parts of the second silicon carbide ingot 16 under the same conditions.
[0227] The output of this comparative example is detailed in Table 6.
[0228] Comparative Example 2:
[0229] Compared with Example 1-1, the main differences of Comparative Example 2 are: the load natural frequency is 18.7KHz; the spacing of the vertical path and the spacing of the parallel path are 400μm; the amplitude of the ultrasonic wave is 5μm; and the output power of the ultrasonic wave is 600w.
[0230] The scanning interval of the laser 4 is 400 μm, which is beyond the scope of the present invention, resulting in the peeling of the upper and lower parts of the second silicon carbide ingot 16 when the output power and amplitude of the ultrasonic wave are increased, causing the silicon carbide wafer to break.
[0231] The output of this comparative example is detailed in Table 6.
[0232] Comparative Example 3:
[0233] Compared with Example 1-1, the main differences of Comparative Example 3 are: the preset speed is 800 mm / s; the load natural frequency is 18.6 KHz; the amplitude of the ultrasonic wave is 11 μm; and the output power of the ultrasonic wave is 800 w.
[0234] The platform moving speed is too fast, which exceeds the scope of this patent, resulting in failure to obtain a good modified layer 5, which causes difficulties in subsequent peeling. When the output power and amplitude of the ultrasonic wave are increased, the upper and lower parts of the second silicon carbide ingot 16 are peeled off, resulting in the fragmentation of the silicon carbide wafer.
[0235] The output of this comparative example is detailed in Table 6.
[0236] Comparative Example 4:
[0237] Compared with Example 1-1, the main differences of Comparative Example 4 are: the spacing of the vertical path and the spacing of the parallel path are 400 μm; the output power of the ultrasonic wave is 10 w.
[0238] Since the ultrasonic energy is insufficient to expand and fully connect the cracks in the modified layer 5, the upper and lower parts of the second silicon carbide ingot 16 cannot be separated, resulting in internal damage and breakage.
[0239] The output of this comparative example is detailed in Table 6.
[0240] Comparative Example 5:
[0241] Compared with Example 1-1, the main differences of Example 5 are: the pulse width of laser 4 is 10ps; the spacing of the vertical path and the spacing of the parallel path are 400μm; the load natural frequency is 18.7KHz; the amplitude of the ultrasonic wave is 5μm; and the output power of the ultrasonic wave is 50w.
[0242] Since the energy of the single-pulse laser 4 is insufficient to expand and fully connect the cracks in the modified layer 5, the upper and lower parts of the second silicon carbide ingot 16 cannot be separated, resulting in internal damage and breakage.
[0243] The output of this comparative example is detailed in Table 6.
[0244] Comparative Example 6
[0245] Compared with Example 1-1, the main differences of Comparative Example 6 are: the pulse width of laser 4 is 10ns; the preset speed is 800mm / s; the load natural frequency is 18.6KHz; the amplitude of the ultrasonic wave is 11μm; and the output power of the ultrasonic wave is 60w.
[0246] Since the energy of the single-pulse laser 4 is too large and the ideal modified layer 5 is not formed, the upper part and the lower part of the second silicon carbide ingot 16 cannot be separated, resulting in internal damage and breakage.
[0247] The output of this comparative example is detailed in Table 6.
[0248] Comparative Example 7:
[0249] Compared with Example 1-1, the main differences of Comparative Example 7 are: the thickness of the first silicon carbide ingot 1 is 10 mm; the spacing of the vertical paths or the spacing of the parallel paths is 400 μm; the load natural frequency is 80.8 KHz; and the output power of the ultrasonic wave is 10 W.
[0250] In Comparative Example 7, an inappropriate ultrasonic generator 8 was selected, resulting in that the upper portion and the lower portion of the second silicon carbide ingot 16 could not be separated.
[0251] The output of this comparative example is detailed in Table 6.
[0252] Comparative Example 8:
[0253] Compared with Example 1-1, the main differences of Comparative Example 8 are: the thickness of the first silicon carbide ingot 1 is 10 mm; the pulse width of the laser 4 is 10 ps; the spacing of the vertical path or the spacing of the parallel path is 400 μm; the load natural frequency is 81.3 KHz; the output frequency of the ultrasonic generator 8 is 40 KHz; the amplitude of the ultrasonic wave is 5 μm; and the output power of the ultrasonic wave is 50 W.
[0254] In Comparative Example 8, an inappropriate ultrasonic generator 8 was selected, resulting in that the upper portion and the lower portion of the second silicon carbide ingot 16 could not be separated.
[0255] The output of this comparative example is detailed in Table 6.
[0256] Comparative Example 9
[0257] Compared with Example 1-1, the main differences of Comparative Example 9 are: the thickness of the first silicon carbide ingot 1 is 10 mm; the pulse width of the laser 4 is 10 ns; the preset speed is 800 mm / s; the load natural frequency is 80.9 KHz; the output frequency of the ultrasonic generator 8 is 60 KHz; the amplitude of the ultrasonic wave is 11 μm; and the output power of the ultrasonic wave is 60 W.
[0258] In Comparative Example 9, an inappropriate ultrasonic generator 8 was selected, resulting in that the upper portion and the lower portion of the second silicon carbide ingot 16 could not be separated.
[0259] The output of this comparative example is detailed in Table 6.
[0260] Table 1 Output of Examples 1-1 to 1-8
[0261]
[0262]
[0263] Table 2 Output of Examples 2 to 6 and Examples 10 to 12
[0264]
[0265]
[0266] Table 3 Output of Examples 7-1 to 7-8
[0267]
[0268]
[0269] Table 4 Output of Examples 8-1 to 8-8
[0270]
[0271] Table 5 Output of Examples 9-1 to 9-8
[0272]
[0273] Table 6 Output of Comparative Examples 1 to 9
[0274]
[0275]
[0276] In the above table: Φ: diameter of the first silicon carbide ingot; H: thickness of the first silicon carbide ingot; A: wavelength of laser; d: sum of thickness of silicon carbide wafer and preset grinding amount; e: spot diameter of laser; f: pulse width of laser; P: power of laser; V: preset speed; L: spacing of vertical paths or spacing of parallel paths; I: natural frequency of load; F: output frequency of ultrasonic generator; G: amplitude of ultrasonic wave; K: output power of ultrasonic wave; T: time of resonance between ultrasonic wave and upper part of second silicon carbide ingot; X: distance between lower part of second silicon carbide ingot and supporting platform; Y: thickness removed by grinding of third silicon carbide ingot; Z: thickness removed by grinding of fourth silicon carbide ingot; p: frequency of laser irradiation; M: number of silicon carbide wafers produced by the method of the present invention; N: number of silicon carbide wafers produced by conventional multi-wire cutting; Q: increased yield of the method of the present invention compared with conventional method; Q=(MN) / N.
[0277] M is determined by H, d, e, Y and Z. Specifically, M = H / (d+e+Y+Z). N is determined by H and the traditional wire cutting diameter and thickness processing allowance. Generally, 3 silicon carbide wafers are produced for every 2mm ingot, which can be used as the basic data for calculation.
[0278] The present invention combines the laser stealth cutting technology with the ultrasonic stripping technology, uses the laser stealth cutting to cut the first silicon carbide ingot, generates a specific modified layer inside the first silicon carbide ingot, and obtains the second silicon carbide ingot; then uses the ultrasonic resonance principle to physically strip the upper and lower parts of the second silicon carbide ingot after the laser stealth cutting. The cutting method provided by the present invention has a fast stripping speed, and the stripping process does not exceed 2 seconds. The rough silicon carbide wafer after stripping is complete and can enter the subsequent normal substrate processing steps to process qualified silicon carbide substrate products. At the same time, the third silicon carbide ingot after stripping is complete, and the surface finish of the silicon carbide ingot to be cut obtained after thinning and grinding is high, and laser stealth cutting can be performed again to strip the second rough silicon carbide wafer, which is repeated in sequence, and finally the high-efficiency and low-cost cutting of silicon carbide ingots can be achieved. Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, substitute and modify the above embodiments within the scope of the invention without departing from the principles and purpose of the present invention. All such changes should fall within the scope of protection of the claims of the present invention.
Claims
1. A method for cutting a silicon carbide ingot, characterized in that: include: irradiating the upper surface of the first silicon carbide ingot with a laser to form a modified layer inside the first silicon carbide ingot to obtain a second silicon carbide ingot, wherein the modified layer divides the second silicon carbide ingot into an upper part and a lower part; Obtaining a load natural frequency of the second silicon carbide ingot; adhering the upper surface of the second silicon carbide ingot to an ultrasonic generator; The output frequency of the ultrasonic generator is set according to the load natural frequency and the ultrasonic generator is started to separate the upper part and the lower part of the second silicon carbide ingot to obtain a silicon carbide wafer.
2. The method for cutting a silicon carbide ingot according to claim 1, characterized in that: The step of starting the ultrasonic generator to separate the upper portion and the lower portion of the second silicon carbide ingot to obtain a silicon carbide wafer comprises: Starting the ultrasonic generator so that the ultrasonic wave generated by the ultrasonic generator resonates with the upper portion of the second silicon carbide ingot; After the ultrasonic wave resonates with the upper part of the second silicon carbide crystal ingot for a set time, the upper part and the lower part of the second silicon carbide crystal ingot are separated to obtain a rough silicon carbide wafer and a third silicon carbide crystal ingot, wherein the lower surface of the rough silicon carbide wafer is a first damaged layer; The rough silicon carbide wafer is processed to obtain the silicon carbide wafer.
3. The method for cutting a silicon carbide ingot according to claim 2, characterized in that: The step of processing the rough silicon carbide wafer to obtain the silicon carbide wafer comprises: Using a first grinding device to perform a thinning and grinding process on the lower surface of the rough silicon carbide wafer to remove the first damaged layer, thereby obtaining the silicon carbide wafer; Wherein, the grinding amount of the rough silicon carbide wafer is 30-70 μm.
4. The method for cutting a silicon carbide ingot according to claim 2, characterized in that: The cutting method further comprises: Using a second grinding device to perform a thinning and grinding process on the upper surface of the third silicon carbide crystal ingot to obtain a fourth silicon carbide crystal ingot; Using a third grinding device to perform a thinning and grinding process on the upper surface of the fourth silicon carbide ingot to obtain a silicon carbide ingot to be cut; Wherein, the upper surface of the third silicon carbide ingot is a second damaged layer, and the thickness of the second damaged layer is 20-50 μm.
5. The method for cutting a silicon carbide ingot according to claim 4, characterized in that: The mesh number of the second grinding device is smaller than the mesh number of the third grinding device; and / or The grinding depth of the third silicon carbide crystal ingot is 30-60 μm, and the surface finish of the fourth silicon carbide crystal ingot is 12-15 nm; and / or The grinding amount of the fourth silicon carbide ingot is 10-30 μm, and the surface finish of the silicon carbide ingot to be cut is 2-5 nm; and / or The set time is 1 to 2 seconds; and / or, The output frequency of the ultrasonic generator is 90%*load natural frequency to 110%*load natural frequency; and / or, The amplitude of the ultrasonic wave is 3 to 10 μm; and / or, The output power of the ultrasonic generator is 20-500W.
6. The method for cutting a silicon carbide ingot according to claim 2, wherein obtaining a rough silicon carbide wafer comprises: After the upper and lower parts of the second silicon carbide ingot are separated, the ultrasonic generator is turned off, and the ultrasonic vibrator with the rough silicon carbide wafer attached thereto is placed in a water tank; Injecting degumming liquid into the water tank so that the degumming liquid submerges the ultrasonic vibrator and the rough silicon carbide wafer; The degumming liquid is heated to separate the ultrasonic vibration head from the rough silicon carbide wafer.
7. The method for cutting a silicon carbide ingot according to claim 1, characterized in that: The step of irradiating the upper surface of the first silicon carbide ingot with laser light comprises: vertically arranging a laser emitter above the first silicon carbide ingot, focusing the laser emitted by the laser emitter on the inside of the first silicon carbide ingot, and controlling the laser emitter to move along a preset path at a preset speed; Wherein, the distance between the position where the laser is focused inside the first silicon carbide ingot and the upper surface of the first silicon carbide ingot is the sum of the thickness of the silicon carbide wafer and a preset grinding amount; and / or, The preset paths include a parallel path group and / or a vertical path group, the parallel path group includes a plurality of parallel paths arranged at equal intervals, the vertical path group includes a plurality of vertical paths arranged at equal intervals, and the parallel paths and the vertical paths are perpendicular to each other; and / or, The distance between two adjacent parallel paths is 60 to 350 μm; and / or, The distance between two adjacent vertical paths is 60 to 350 μm; and / or, The preset speed is 100-600 mm / s; and / or, The wavelength of the laser is 355 to 1080 nm; and / or, The pulse width of the laser is 20ps to 5ns; and / or, The frequency of the laser irradiation is 30 to 40 KHZ; and / or, The cross-sectional area of the modified layer is the same as the cross-sectional area of the first silicon carbide ingot.
8. The method for cutting a silicon carbide ingot according to claim 1, characterized in that: The ultrasonic generator comprises an ultrasonic vibration head, and the diameter of the ultrasonic vibration head is greater than or equal to the diameter of the first silicon carbide ingot; Preferably, the cross-sectional area of the ultrasonic vibrator is 115% to 130% of the cross-sectional area of the first silicon carbide ingot; And / or, adhering the upper surface of the second silicon carbide crystal ingot to the ultrasonic generator includes: providing an adhesive layer between the upper surface of the second silicon carbide crystal ingot and the ultrasonic vibration head.
9. A device for cutting a silicon carbide ingot, characterized in that: include: A laser emitter, configured to emit a laser beam to irradiate the upper surface of the first silicon carbide ingot, so as to form a modified layer inside the first silicon carbide ingot, thereby obtaining a second silicon carbide ingot; A processing device, used for obtaining the load natural frequency of the second silicon carbide ingot; setting the output frequency of the ultrasonic generator according to the load natural frequency, and generating a start signal; An ultrasonic generator is connected to the processing equipment and is used to generate ultrasonic waves after the upper surface of the second silicon carbide ingot adheres to the ultrasonic generator and receives the start signal, so as to separate the upper and lower parts of the second silicon carbide ingot to obtain a silicon carbide wafer.
10. The silicon carbide ingot cutting device according to claim 9, characterized in that: The ultrasonic generator comprises: a generator body and an ultrasonic vibration head, wherein the generator body is used to generate ultrasonic waves; the ultrasonic vibration head is arranged at the output end of the generator body, and is used to transmit the vibration energy of the ultrasonic wave to the second silicon carbide ingot, so as to obtain a rough silicon carbide wafer and a third silicon carbide ingot; The silicon carbide ingot cutting device further includes a receiving platform, which is disposed directly below the ultrasonic vibration head and is used to receive the third silicon carbide ingot that falls off from the ultrasonic vibration head.
Citation Information
Patent Citations
SiC WAFER PRODUCING METHOD
CN108447783A
Wafer making process and wafer making equipment
CN110277349A
Low-loss silicon carbide crystal ingot laser slicing method
CN117139865A
Crystal ingot stripping device assisted by torsional ultrasonic vibration and using method of crystal ingot stripping device
CN117594422A
Production method of wafer
JP2016225534A
Cited By
Composite silicon carbide substrate fragmentation method
CN121487518A