Cutting method of silicon carbide crystal

By combining the metal cutting lines with diamond abrasive particles on the surface with mortar containing diamond powder, the cutting process parameters are optimized, and the problem of high loss of silicon carbide cutting is solved, low loss and high quality cutting effect is achieved, and the Production cost.

CN118906274APending Publication Date: 2024-11-08BEIJING TIANKE HEDA SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411334885.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The high loss problem caused by existing silicon carbide cutting methods has led to high production costs.

Method used

The metal cutting lines with diamond abrasive particles on the surface are combined with the mortar containing diamond powder. By optimizing cutting process parameters such as line diameter, tension, speed and swing angle, the cutting loss of silicon carbide crystal is reduced.

Benefits of technology

The cutting loss rate of silicon carbide is significantly reduced, from 16.7% to 5.8%, which improves the sheet yield, reduces production costs, and ensures cutting quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118906274A_ABST
    Figure CN118906274A_ABST
Patent Text Reader

Abstract

The invention provides a silicon carbide crystal cutting method which comprises the following steps: carrying out mortar cutting treatment on a silicon carbide crystal by using cutting equipment provided with a cutting line to obtain a silicon carbide wafer; the cutting line is a metal line of which the surface is electroplated with diamond abrasive particles; the wire diameter of the cutting wire is 20-70 [mu] m; mortar adopted in the mortar cutting treatment comprises diamond micro-powder and cutting oil; the viscosity of the mortar is 5 to 50 mPas. Compared with the prior art, through the combined action of the cutting line electroplated with the diamond abrasive particles and the mortar liquid containing the diamond micro-powder and the combination of the setting of cutting process parameters, the change of the total thickness and the change of the warping degree of the cut silicon carbide wafer are ensured; therefore, the purpose of reducing the cutting loss by adopting thinner cutting lines and abrasive particles with smaller granularity is achieved, and the loss of a single cut silicon carbide crystal is reduced to be less than 100 microns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor technology, and in particular relates to a method for cutting a silicon carbide crystal. Background Art

[0002] Silicon carbide crystals are widely used in semiconductors, electronic components and other fields. They have high hardness. For components that require thinner size, large-sized silicon carbide crystals need to be cut.

[0003] At present, mortar cutting is still the most common method for cutting silicon carbide, and a small part of it is cut with diamond wire. However, due to the high hardness of silicon carbide, the diameter of the cutting wire and the diameter of the mortar abrasive used in cutting are relatively large, resulting in high losses when cutting silicon carbide crystals. The cutting loss of a single piece is more than 100 μm. For a wafer with a target slice thickness of 500 μm, the cutting loss of a single piece is more than 16.7%. The large cutting loss leads to high production costs of silicon carbide wafers. Therefore, reducing the cutting loss of silicon carbide is of great significance to reducing the production cost of silicon carbide. Summary of the invention

[0004] In view of this, the technical problem to be solved by the present invention is to provide a low-loss cutting method for silicon carbide crystals.

[0005] The present invention provides a method for cutting a silicon carbide crystal, comprising the following steps:

[0006] Using a cutting device equipped with a cutting wire to perform a slurry cutting process on a silicon carbide crystal to obtain a silicon carbide wafer; the cutting wire is a metal wire with diamond abrasive grains electroplated on the surface; the wire diameter of the cutting wire is 20-70 μm;

[0007] The mortar used in the mortar cutting process includes diamond micropowder and cutting oil;

[0008] The viscosity of the mortar is 5-50 mPa•s.

[0009] Preferably, the diamond abrasive has a particle size of 3-10 μm.

[0010] Preferably, the particle size of the diamond powder is 5.5-15 μm; the mass of the diamond powder is 2%-20% of the mass of the mortar.

[0011] Preferably, the tension of the cutting line during the mortar cutting process is 1-10 N.

[0012] Preferably, the linear speed of the cutting line during the mortar cutting process is 10-24 m / s.

[0013] Preferably, the swing angle of the silicon carbide crystal during the mortar cutting process is 0.5° to 7°;

[0014] The cutting wire is a tungsten wire with diamond abrasive grains electroplated on the surface.

[0015] Preferably, the relationship between the wire diameter of the cutting wire and the tension of the cutting wire during mortar cutting satisfies (10-20) micrometers: 1 N.

[0016] Preferably, the ratio of the particle size of the diamond abrasive to the wire diameter of the cutting wire is 1:(6-10);

[0017] The relationship between the wire diameter of the cutting wire and the wire speed of the cutting wire during the mortar cutting process satisfies 70 μm: 12 m / s to 20 μm: 24 m / s.

[0018] Preferably, the flow rate of the mortar used in the mortar cutting process is 1000~4000 L / min.

[0019] Preferably, the total thickness variation of the silicon carbide wafer is less than or equal to 15 μm; the warpage of the silicon carbide wafer is less than or equal to 35 μm; and the cutting loss of the silicon carbide wafer is less than 100 μm.

[0020] The present invention provides a method for cutting silicon carbide crystals, comprising the following steps: using a cutting device equipped with a cutting wire to perform a slurry cutting process on a silicon carbide crystal to obtain a silicon carbide wafer; the cutting wire is a metal wire with diamond abrasive grains electroplated on the surface; the wire diameter of the cutting wire is 20-70 μm; the slurry used in the slurry cutting process includes diamond micropowder and cutting oil; the viscosity of the slurry is 5-50 mPa•s. Compared with the prior art, the present invention ensures the total thickness change and warpage change of the silicon carbide wafer after cutting by combining the setting of the cutting process parameters with the cutting wire electroplated with diamond abrasive grains and the slurry liquid containing diamond micropowder, thereby achieving the purpose of reducing the cutting loss by using a finer cutting wire and a smaller particle size abrasive grains, and reducing the single-chip loss of the silicon carbide crystal to less than 100 μm.

[0021] Experimental results show that the silicon carbide cutting loss of the cutting method provided by the present invention is 31~100 μm, which is significantly lower than the current level in the silicon carbide cutting industry. The loss rate is reduced from more than 16.7% to a minimum of 5.8%, which greatly saves silicon carbide crystal materials, greatly improves the output rate of single-column silicon carbide crystals, reduces the production cost of silicon carbide wafers, and has good cutting quality, with a total thickness change of less than or equal to 15 μm and a warpage of less than or equal to 35 μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of silicon carbide crystal loss. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] The present invention provides a method for cutting a silicon carbide crystal, comprising the following steps: using a cutting device equipped with a cutting wire to perform a mortar cutting process on a silicon carbide crystal to obtain a silicon carbide wafer; the cutting wire is a metal wire with diamond abrasive grains electroplated on the surface; the wire diameter of the cutting wire is 20-70 μm; the mortar used in the mortar cutting process comprises diamond micropowder and cutting oil; and the viscosity of the mortar is 5-50 mPa•s.

[0025] The present invention has no particular limitation on the sources of all raw materials, and any raw materials available on the market can be used.

[0026] According to the present invention, the cutting wire is a metal wire with diamond abrasive grains electroplated on the surface; the particle size of the diamond abrasive grains is preferably 3-10 μm; in some embodiments provided by the present invention, the particle size of the diamond abrasive grains is specifically 10 μm, 6 μm or 3 μm; the wire diameter of the cutting wire is 20-70 μm; in some embodiments provided by the present invention, the wire diameter of the cutting wire is specifically 70 μm, 50 μm, 30 μm or 10 μm; in a specific embodiment provided by the present invention, the cutting wire is a tungsten wire with diamond abrasive grains electroplated on the surface. As the cutting wire diameter decreases, the cutting ability will decrease, resulting in poor cutting quality, especially when the wire diameter is less than 100 μm, the cutting wire tension drops sharply, and the use of high-strength tungsten wire can compensate for the decrease in cutting tension caused by the decrease in wire diameter to a certain extent.

[0027] According to the present invention, the ratio of the particle size of the diamond abrasive to the wire diameter of the cutting wire is preferably 1:(6-10); in some embodiments provided by the present invention, the ratio of the particle size of the diamond abrasive to the wire diameter of the cutting wire is specifically 1:7, 1:8.3, 1:10 or 1:6.6.

[0028] According to the present invention, the mortar used in the mortar cutting process includes diamond micropowder and cutting oil; the particle size of the diamond micropowder is preferably 5.5~15 μm, more preferably 5.5~12 μm, and more preferably 5.5~10 μm; in some embodiments provided by the present invention, the particle size of the diamond micropowder is specifically 5.5 μm, 8 μm or 10 μm; the mass of the diamond micropowder is preferably 2%~20% of the mass of the mortar, more preferably 5%~20%; in some embodiments provided by the present invention, the mass of the diamond micropowder is specifically 5%, 10%, 18% or 20% of the mass of the mortar; the viscosity of the mortar is preferably 5~50 mPa•s, more preferably 9~50 mPa•s (temperature: 25°C, rotor: 1#, rotation speed: 60 rpm); in some embodiments provided by the present invention, the viscosity of the mortar is specifically 9 mPa·s, 18 mPa·s, 45 mPa·s or 50 mPa·s.

[0029] According to the present invention, the wire diameter of the cutting wire and the viscosity of the mortar preferably satisfy the relationship of 70 μm: 9 mPa•s ~ 20 μm: 50 mPa•s; that is, the larger the wire diameter of the cutting wire, the smaller the viscosity of the mortar; in some embodiments provided by the present invention, the wire diameter of the cutting wire and the viscosity of the mortar specifically satisfy the relationship of 70 μm: 9 mPa•s, 50 μm: 18 mPa•s, 30 μm: 45 mPa•s or 20 μm: 50 mPa•s.

[0030] A silicon carbide crystal is subjected to mortar cutting treatment using a cutting device equipped with a cutting wire to obtain a silicon carbide wafer; the cutting device can be a cutting device well known to those skilled in the art, without any special restrictions, and a multi-wire saw is preferably used in the present invention; the silicon carbide crystal can be a silicon carbide crystal well known to those skilled in the art, without any special restrictions, and in the present invention, the diameter of the silicon carbide crystal is preferably 100-200 mm, more preferably 150 mm; the thickness of the silicon carbide crystal is preferably 10-50 mm, more preferably 20-40 mm, and even more preferably 30 mm.

[0031] The loss of silicon carbide crystals mainly comes from the diameter of the cutting wire and the grinding loss of the slurry during the cutting process, see Figure 1 , Figure 1The figure is a schematic diagram of silicon carbide crystal loss, total loss = cutting wire diameter + 2 × diamond powder particle size in the mortar, that is, the cutting loss of the present invention is 31~100 μm. As the cutting wire diameter decreases, the cutting ability will decrease, resulting in poor cutting quality. In particular, when the wire diameter is lower than 100 μm, the cutting wire tension drops sharply. The use of high-strength tungsten wire can compensate for the decrease in cutting tension caused by the decrease in wire diameter to a certain extent. However, due to the high hardness of silicon carbide material, the cutting quality cannot be ensured by improving the cutting wire material alone. Therefore, the cutting wire electroplated with diamond abrasives and the mortar containing diamond powder work together, combined with the setting of cutting process parameters (such as wire tension, wire speed, swing angle, cutting time), to ensure the total thickness change and warpage change of silicon carbide wafers after cutting.

[0032] According to the present invention, the tension of the cutting line during the mortar cutting process is preferably 1-10 N, more preferably 1-8 N, and even more preferably 1-7 N; in some embodiments provided by the present invention, the tension of the cutting line during the mortar cutting process is specifically 7 N, 4 N, 2.5 N or 1 N.

[0033] According to the present invention, further specifically, the relationship between the wire diameter of the cutting line and the tension of the cutting line during mortar cutting treatment preferably satisfies (10~20) microns: 1 N; in some embodiments provided by the present invention, the relationship between the wire diameter of the cutting line and the tension of the cutting line during mortar cutting treatment specifically satisfies 10 microns: 1 N, 12.5 microns: 1 N, 12 microns: 1 N or 20 microns: 1 N.

[0034] According to the present invention, the linear speed of the cutting line during the mortar cutting process is preferably 10-24 m / s; in some embodiments provided by the present invention, the linear speed of the cutting line during the mortar cutting process is specifically 12 m / s, 18 m / s or 24 m / s.

[0035] According to the present invention, further specifically, the relationship between the wire diameter of the cutting line and the linear speed of the cutting line during the mortar cutting process preferably satisfies 70 μm: 12 m / s~20 μm: 24 m / s, that is, the larger the wire diameter of the cutting line, the smaller the linear speed during the cutting process; in some embodiments provided by the present invention, the relationship between the wire diameter of the cutting line and the linear speed of the cutting line during the mortar cutting process satisfies 70 μm: 12 m / s, 50 μm: 18 m / s, 30 μm: 24 m / s or 20 μm: 24 m / s.

[0036] According to the present invention, the rocking angle of the silicon carbide crystal during the mortar cutting treatment is preferably 0.5°~7°, more preferably 1°~5°, and even more preferably 1°~3°; in some embodiments provided by the present invention, the rocking angle of the silicon carbide crystal during the mortar cutting treatment is specifically 3° or 1°.

[0037] According to the present invention, during the mortar cutting process, the mortar flow rate is preferably 1000L / min~4000L / min; in some embodiments provided by the present invention, during the mortar cutting process, the mortar flow rate is specifically 4000 L / min, 3000 L / min, 2000 L / min or 1000 L / min.

[0038] According to the present invention, more specifically, during the mortar cutting process, the flow rate of the mortar is inversely proportional to the viscosity of the mortar, that is, the smaller the viscosity of the mortar, the larger the flow rate.

[0039] According to the present invention, more specifically, during the mortar cutting process, the flow rate of the mortar is inversely proportional to the linear speed of the cutting line, that is, the greater the linear speed of the cutting line, the smaller the flow rate of the mortar.

[0040] According to the present invention, the total time of the mortar cutting treatment is preferably 50 to 120 h, more preferably; in some embodiments provided by the present invention, the total time of the mortar cutting treatment is specifically 50 h, 80 h, 100 h or 120 h.

[0041] According to the present invention, the total thickness variation of the silicon carbide wafer is less than or equal to 15 μm; the warpage of the silicon carbide wafer is less than or equal to 35 μm; and the cutting loss of the silicon carbide wafer is less than 100 μm.

[0042] The present invention ensures the total thickness change and warpage change of the silicon carbide wafer after cutting by combining the cutting wire electroplated with diamond abrasive grains and the slurry containing diamond micropowder, and setting the cutting process parameters, so as to achieve the purpose of reducing the cutting loss by using a finer cutting wire and abrasive grains of smaller particle size, and reduce the single-chip loss of the silicon carbide crystal cutting to less than 100 μm.

[0043] In order to further illustrate the present invention, a method for cutting a silicon carbide crystal provided by the present invention is described in detail below in conjunction with embodiments.

[0044] The reagents used in the following examples are all commercially available.

[0045] Example 1

[0046] 1.1 Diamond abrasive wire with diamond abrasive grains electroplated on the surface is selected as the cutting wire, wherein the cutting wire material is metal tungsten (the wire diameter of the main wire is 50 μm), the surface is electroplated with diamond abrasive grains, the abrasive grain size range is 10 microns, and the cutting wire diameter range is 70 μm;

[0047] 1.2 Diamond micropowder with a particle size of 5.5 microns was fully mixed with cutting oil to form a mortar, wherein the mass proportion of diamond micropowder was 5%, and the viscosity of the mixed mortar was 9 mPa·s;

[0048] 1.3 Using mature multi-wire cutting equipment, load the above-mentioned cutting wire and mortar into the equipment to cut silicon carbide crystals with a diameter of 150 mm and a thickness of 30 mm;

[0049] 1.4 According to the type of cutting wire used and the concentration of mortar, the multi-wire sawing machine sets the cutting wire tension to 7 N, the cutting wire speed to 12 m / s, the swing angle to 3° during crystal cutting, the mortar flow rate to 4000 L / min, and the total cutting time to 50 h;

[0050] After 1.5 cutting, a silicon carbide wafer was obtained, the total thickness change of the wafer was 8.3 μm, the warpage of the wafer was 20.2 μm, and the single-piece cutting loss was 81 μm.

[0051] Example 2

[0052] 2.1 Diamond wire with diamond abrasive grains electroplated on the surface is selected as the cutting wire, where the cutting wire is made of metal tungsten (the wire diameter of the main wire is 38 μm), the surface is electroplated with diamond abrasive grains, the abrasive grain size range is 6 microns, and the cutting wire diameter range is 50 μm;

[0053] 2.2 Diamond micropowder with a particle size of 8 microns was fully mixed with cutting oil to form a mortar, wherein the mass proportion of diamond micropowder was 10%, and the viscosity of the mixed mortar was 18 mPa·s;

[0054] 2.3 Using mature multi-wire cutting equipment, load the above-mentioned cutting wire and mortar into the equipment to cut silicon carbide crystals with a diameter of 150 mm and a thickness of 30 mm;

[0055] 2.4 According to the type of cutting wire used and the concentration of mortar, the multi-wire sawing machine sets the cutting wire tension to 4 N, the cutting wire speed to 18 m / s, the swing angle to 3° during crystal cutting, the mortar flow rate to 3000 L / min, and the total cutting time to 80 h;

[0056] After 2.5 cutting, a silicon carbide wafer was obtained. The total thickness change of the wafer was 10.6 μm, the warpage of the wafer was 28.7 μm, and the single-piece cutting loss was 66 μm.

[0057] Example 3

[0058] 3.1 Diamond wire with diamond abrasive grains electroplated on the surface is selected as the cutting wire, wherein the cutting wire material is metal tungsten (the wire diameter of the main wire is 24 μm), the surface is electroplated with diamond abrasive grains, the abrasive grain size range is 3 microns, and the cutting wire diameter range is 30 μm;

[0059] 3.2 Diamond micropowder with a particle size of 10 microns was fully mixed with cutting oil to form a mortar, in which the mass proportion of diamond particles was 18%, and the viscosity of the mixed mortar was 45 mPa·s;

[0060] 3.3 Using mature multi-wire cutting equipment, load the above-mentioned cutting wire and mortar into the equipment to cut silicon carbide crystals with a diameter of 150 mm and a thickness of 30 mm;

[0061] 3.4 According to the type of cutting wire used and the concentration of mortar, the multi-wire sawing machine sets the cutting wire tension to 2.5 N, the cutting wire speed to 24 m / s, the swing angle to 3° during crystal cutting, the mortar flow rate to 2000 L / min, and the total cutting time to 100 h;

[0062] After 3.5 cutting, the silicon carbide wafer was obtained. The total thickness change of the wafer was 13.2 μm, the warpage of the wafer was 29.3 μm, and the single-piece cutting loss was 50 μm.

[0063] Example 4

[0064] 4.1 Diamond wire with diamond abrasive grains electroplated on the surface is selected as the cutting wire, wherein the cutting wire material is metal tungsten (the wire diameter of the main wire is 14 μm), the surface is electroplated with diamond abrasive grains, the abrasive grain size range is 3 microns, and the cutting wire diameter range is 20 μm;

[0065] 4.2 Diamond micropowder with a particle size of 5.5 microns was fully mixed with cutting oil to form a mortar, in which the mass proportion of diamond particles was 20%, and the viscosity of the mixed mortar was 50 mPa·s;

[0066] 4.3 Using mature multi-wire cutting equipment, load the above-mentioned cutting wire and mortar into the equipment to cut silicon carbide crystals with a diameter of 150 mm and a thickness of 30 mm;

[0067] 4.4 According to the type of cutting wire used and the concentration of mortar, the multi-wire sawing machine sets the cutting wire tension to 1 N, the cutting wire speed to 24 m / s, the swing angle to 1° during crystal cutting, the mortar flow rate to 1000 L / min, and the total cutting time to 120 h;

[0068] After 4.5 cutting, a silicon carbide wafer was obtained, the total thickness change of the wafer was 13.9 μm, the warpage of the wafer was 33.7 μm, and the single-piece cutting loss was 31 μm.

[0069] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for cutting a silicon carbide crystal, characterized in that: The following steps are involved: Using a cutting device equipped with a cutting wire to perform a slurry cutting process on a silicon carbide crystal to obtain a silicon carbide wafer; the cutting wire is a metal wire with diamond abrasive grains electroplated on the surface; the wire diameter of the cutting wire is 20-70 μm; The mortar used in the mortar cutting process includes diamond micropowder and cutting oil; The viscosity of the mortar is 5-50 mPa•s.

2. The cutting method according to claim 1, characterized in that: The particle size of the diamond abrasive grains is 3-10 μm.

3. The cutting method according to claim 1, characterized in that: The particle size of the diamond micropowder is 5.5-15 μm; the mass of the diamond micropowder is 2%-20% of the mass of the mortar.

4. The cutting method according to claim 1, characterized in that: The tension of the cutting line during the mortar cutting process is 1-10 N.

5. The cutting method according to claim 1, characterized in that: The linear speed of the cutting line during the mortar cutting process is 10-24 m / s.

6. The cutting method according to claim 1, characterized in that: The swing angle of the silicon carbide crystal during the mortar cutting process is 0.5°~7°; The cutting wire is a tungsten wire with diamond abrasive grains electroplated on the surface.

7. The cutting method according to claim 1, characterized in that: The relationship between the wire diameter of the cutting wire and the tension of the cutting wire during mortar cutting satisfies (10-20) microns: 1 N.

8. The cutting method according to claim 1, characterized in that: The ratio of the particle size of the diamond abrasive to the wire diameter of the cutting wire is 1:(6-10); The relationship between the wire diameter of the cutting wire and the wire speed of the cutting wire during the mortar cutting process satisfies 70 μm: 12 m / s to 20 μm: 24 m / s.

9. The cutting method according to claim 1, characterized in that: The flow rate of the mortar used in the mortar cutting process is 1000~4000 L / min.

10. The cutting method according to claim 1, characterized in that: The total thickness variation of the silicon carbide wafer is less than or equal to 15 μm; the warpage of the silicon carbide wafer is less than or equal to 35 μm; and the cutting loss of the silicon carbide wafer is less than 100 μm.