Composite material compression roller forming method and compression roller for lithium ion battery roller press
By adopting carbon fiber composite material, the problem of large weight and high energy consumption of aluminum alloy rollers in lithium-ion battery electrode rolling equipment is solved, and the roller pressure effect with high precision and low energy consumption is achieved, which improves the electrode rolling effect Quality and equipment performance.
Patent Information
- Application Number
- CN202411232249.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-08
AI Technical Summary
The aluminum alloy rollers in the existing lithium-ion battery plate roller pressing equipment have problems such as large weight, slow starting speed, high energy consumption, large raw material loss, and large roller jump and roll curvature, resulting in uneven coating thickness and compaction. Uneven density affects the quality of the pole sheet.
By using the composite material press roller molding method, by winding the carbon fiber impregnated resin glue solution, the winding tension, longitudinal winding angle, layer thickness and resin glue content are controlled to form a lightweight and high-rigid carbon fiber composite roller body, and the roller is on the roller. Connecting structures and cladding layers are provided at both ends of the body to perform surface treatment and dynamic balance to ensure high accuracy and stability of the roller body.
It realizes the high strength, low density, high temperature resistance and fatigue resistance of carbon fiber composite rollers, reduces the energy consumption and inertia of the equipment, improves the roller quality and service life of the equipment, and meets the high level of lithium-ion battery roller presses. Accuracy and high efficiency requirements.
Smart Images

Figure CN118906525A_ABST
Abstract
Description
Technical Field
[0001] The invention patent relates to the field of rolling equipment, and in particular to a composite material rolling forming method and a roller for a lithium-ion battery rolling machine. Background Art
[0002] In the production process of lithium-ion batteries, the coated pole pieces need to be rolled to enhance the bonding strength between the coating material and the foil material, and reduce the possibility of the pole pieces falling off during the cycle. In addition, rolling can also make the contact between the active material and the conductive agent particles closer, thereby improving the electronic conductivity. Since the rolling accuracy of the pole pieces is required to be high, the rolling machine needs to have the characteristics of light weight, uniform pressure, easy adjustment, and high precision.
[0003] Currently, aluminum alloy rollers are mostly used in lithium battery pole piece rolling equipment. However, aluminum alloy rollers have obvious defects. They are heavy, slow to start up, have large inertia, consume a lot of energy, and cause large losses of raw materials. When the aluminum alloy roller has large roll jump and roll curvature, the rolling pressure is fed back to the pole piece, causing uneven coating thickness, that is, uneven coating compaction density, which directly affects the pole piece rolling quality. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a composite material roller forming method and a roller for a lithium ion battery roller press.
[0005] In order to solve the problems in the prior art, the invention discloses a composite material roller forming method and a roller for a lithium ion battery roller press.
[0006] In a first aspect, the present invention discloses a composite material roll forming method, comprising: After impregnating a number of bundles of carbon fibers with resin glue, they are wound on a mold. During the winding process, the carbon fiber winding tension, longitudinal winding angle, thickness of a single continuous longitudinal winding layer and content of resin glue are all controlled within a preset range, and the thickness ratio of the longitudinal / circumferential layers is a preset value to form a roller body; A high temperature resistant film is provided on the outside of the roller body; Heating and curing the roller body until the curing degree of the roller body reaches a preset range; Separating the cured roller body from the high temperature resistant film, and separating the cured roller body from the mold to form a composite material roller body; Connecting structures are arranged at both ends of the composite material roller body; The composite material roller body and the connection structure are subjected to surface treatment and dynamic balancing treatment until the surface roughness and circumferential runout detection of the composite material roller body and the connection structure meet preset requirements.
[0007] The technical effects achieved by the above settings are as follows: Carbon fiber has many excellent properties such as high strength, high modulus, high temperature resistance, wear resistance, corrosion resistance, fatigue resistance, and thermal conductivity. Compared with metals such as steel and aluminum, its density is only 1.6g / cm3, which is much lower than the density of aluminum (2.7g / cm3) and steel (7.8g / cm3). Carbon fiber products are lightweight, easy to carry, install and operate, and the energy consumption of carbon fiber products during rotation is greatly reduced. The tensile strength of carbon fiber composite products is as high as 3000MPa or more, and the elastic modulus is 240GPa. They are strong and durable, and their load-bearing and deformation resistance are better than aluminum. In addition, carbon fiber composite products have small inertia, and are used in high-speed rotating equipment to facilitate speed control and effectively reduce shock.
[0008] Furthermore, the carbon fiber winding tension is 70~100N / bundle; the longitudinal winding angle is 10~15°; the thickness of the single continuous longitudinal winding layer does not exceed 4mm; the resin glue content is 10%-20%; and the thickness ratio of the longitudinal / circumferential plies is 20 / 1.
[0009] The technical effect achieved by the above arrangement: improving the rigidity and radial load-bearing capacity of the roller body.
[0010] Furthermore, the curing degree of the roller body reaches more than 90%.
[0011] The technical effect achieved by the above arrangement is: making the roller body sufficiently strong.
[0012] Furthermore, the method of arranging the connection structures at both ends of the composite material roller body is as follows: Cutting both ends of the composite material roll; Ends are pressed into the composite material roller at both ends; Holes are drilled around the contact area between the end head and the composite material roller body, and fasteners are arranged in the holes to fix the end head and the composite material roller body.
[0013] The technical effect achieved by the above arrangement is that the end head is preferably a metal end head, and by adopting the above connection method, the composite material roller body is more securely connected to the connection structure.
[0014] Furthermore, it also includes: before the two ends of the composite material roller body are respectively pressed into the end heads, the contact area between the composite material roller body and the end heads is sandblasted and AB mixed glue is applied.
[0015] The technical effect achieved by the above arrangement is: filling the gap between the composite material roller body and the end head, making the connection between the composite material roller body and the end head tighter and more secure.
[0016] Furthermore, the circular runout detection requirement is: when the rotation speed of the composite material roller reaches 360r / min, the circular runout is ≤0.03mm.
[0017] The technical effects achieved by the above arrangement are: avoiding the movement of the composite material roller, ensuring the rolling quality, and also being able to increase the service life of the composite material roller.
[0018] Furthermore, a composite material coating layer is arranged on the outer side of the composite material roller body.
[0019] The technical effect achieved by the above arrangement is: further improving the smoothness of the surface of the composite material roller.
[0020] Furthermore, the method for setting a composite material coating layer on the outside of the composite material roller body is: using an industrial acetone solution to clean the surface of the composite material roller body, evenly scraping a resin glue on the surface of the composite material roller body, and evenly wrapping the carbon fiber prepreg tape cut according to the designed size onto the surface of the composite material roller body coated with the resin glue, and forming a composite material coating layer after curing.
[0021] The technical effect achieved by the above arrangement is: the composite material coating layer is more tightly connected to the composite material roller body, and bubbles and the like are avoided.
[0022] Furthermore, the method of arranging the high temperature resistant film on the outer side of the roller body is as follows: firstly wrapping the high temperature resistant polytetrafluoroethylene tape on the outer side of the roller body, and then wrapping the glass fiber hoop dry yarn.
[0023] The technical effect achieved by the above settings is: ensuring that during the thermosetting process, excess resin glue overflows as much as possible, the glass fiber hoop dry yarn is used to absorb the resin glue, and the high-temperature resistant polytetrafluoroethylene belt is used to prevent the roller from thermal expansion failure.
[0024] In the second aspect, accordingly, the present invention also provides a roller for a lithium-ion battery roller press, comprising: an end head, a composite material roller body, a fastener and a composite material coating layer; the end head is pressed into the two ends of the composite material roller body, and drill holes are provided around the contact area between the end head and the composite material roller body, and the fastener is screwed into the drill holes; the composite material coating layer is coated on the periphery of the composite material roller body.
[0025] The technical effect achieved by the above settings is: the carbon fiber composite material pressure roller replaces the aluminum alloy pressure roller commonly used in lithium-ion battery roller presses. While improving the roller bearing capacity, reducing the roller weight, and reducing the energy consumption of the equipment, it maintains high-precision coaxiality, shaft end runout, and dynamic balance performance, thereby improving the pole piece rolling quality.
[0026] The present invention has the beneficial effects: The carbon fiber composite material roller is light in weight and easy to carry, install and operate. Compared with metal rollers, the energy consumption of the carbon fiber roller during rotation is greatly reduced, and the roller has small inertia during movement. The speed can be controlled and effectively damped during high-speed rotation. The carbon fiber roller does not deform when used at a temperature of -50°C to 150°C, has high tensile strength and elastic modulus, and has better load-bearing and anti-deformation capabilities than aluminum rollers. The carbon fiber roller obtained by the preparation method of the present invention has a roller circumferential runout of ≤0.03mm and a surface roughness of ≤0.8μm at a rotation speed of 360r / min. When the roller is subjected to a uniformly distributed load of 35kg, the deflection deformation is ≤0.11mm, which can meet the performance requirements of the roller for lithium-ion battery roller press equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the structure of the pressing roller for the lithium ion battery roller press of the present invention.
[0028] Reference numerals: 1. End; 2. Composite material roller body; 3. Fastener; 4. Composite material covering layer. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention. Example
[0030] This embodiment provides a method for forming a composite material roller, which specifically includes the following steps: The composite material roller body is made by impregnating a plurality of bundles of carbon fibers with resin glue on a fiber winding machine and then winding them on a metal mold. The surface of the metal mold is smooth and free of foreign matter and protrusions. The longitudinal winding angle is designed to be 10-15°, and the longitudinal circumferential thickness ratio is designed to be 20 / 1, so as to improve the rigidity and radial load-bearing capacity of the roller body.
[0031] During the winding process, the fiber winding tension needs to be controlled at 70~100N / bundle. Pay attention to scrape off excess epoxy resin glue in time to ensure that the glue content of the roller is controlled at 10%-20%.
[0032] According to the different requirements for roller stiffness and load-bearing capacity in actual application conditions, the longitudinal and circumferential thickness of the roller can be designed to meet the requirements for roller performance under different working conditions.
[0033] After the fiber winding is completed, a layer of glass cloth or glass fiber hoop dry yarn is wound on the surface of the roller body and left to stand for 15-25 minutes to remove excess resin glue in the roller body.
[0034] The above-mentioned glass cloth or glass fiber hoop dry yarn is removed, and a layer of high-temperature resistant polytetrafluoroethylene tape is wound on the surface of the roller body. Then, 4 layers of glass fiber hoop dry yarn are wound on the outside. During the winding process, the tension of the glass fiber hoop dry yarn is controlled at 50~70N / bundle.
[0035] The composite material roller is placed in a heating and curing furnace for rotational heating and curing. It must be ensured that the roller is always in a uniform self-rotation state during the curing process. The curing system is set according to the different resin systems used.
[0036] After curing, when the roller surface temperature drops to room temperature, remove the glass fiber hoop dry yarn and high temperature resistant polytetrafluoroethylene tape, and then perform demoulding to separate the composite roller from the metal mold. According to the design requirements, use the tube cutting equipment to cut off the non-geodesic winding parts at both ends of the cylinder. Generally, the length of the non-geodesic winding area to be cut off is ≥150mm.
[0037] The mating parts of the metal end and the composite roller body are sandblasted and cleaned, and after a layer of AB glue is evenly applied on the contact area of the end and the composite roller body, the metal end is pressed into the composite roller body from both sides using extrusion equipment.
[0038] 4 to 8 threaded holes are processed along the circumference of the contact area between the metal end and the roller body, and countersunk screws with AB glue are screwed into the threaded holes to achieve the fastening and fixation of the metal end and the composite material roller body.
[0039] The composite material roller body and the metal end are rough turned and fine turned until the roller body speed reaches 360r / min and the circumferential runout is ≤0.03mm.
[0040] Furthermore, an industrial acetone solution is used to clean the surface of the composite roller body for fine turning to remove foreign matter such as oil, debris, etc. A thin and uniform layer of resin glue is scraped on the surface of the roller body with a scraper, and the carbon fiber prepreg tape cut to the designed size is evenly wrapped on the roller body surface coated with the resin glue. Note that bubbles are removed in time to form a composite material coating layer.
[0041] The roller body is placed in a vacuum tank using a rotary curing tool for vacuuming, rotating, heating and curing.
[0042] Furthermore, after the surface temperature of the roller coated with the composite material coating layer drops to room temperature, the surface of the roller coated with the composite material coating layer is subjected to secondary finishing until the dynamic balance, circumferential runout and surface roughness of the roller meet the design requirements. Example
[0043] like Figure 1As shown, this embodiment adopts the molding method of the composite material roller described in Example 1 to form a roller for a lithium-ion battery roller press, including: an end head 1, a composite material roller body 2, a fastener 3 and a composite material coating layer 4; the end head 1 is pressed into both ends of the composite material roller body 2, and drill holes are provided around the contact area between the end head 1 and the composite material roller body 2, and the fastener 3 is screwed into the drill holes; the composite material coating layer 4 is coated on the periphery of the composite material roller body 2; the end head 1 is a metal end head, and the fastener 3 is a fastening screw.
[0044] It should be noted that, in this article, relational terms such as first and second are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. At the same time, in the description of the present invention, it should be understood that the orientation or position relationship indicated by the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like are based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the equipment or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. And in the drawings of the present invention, the filling pattern is only to distinguish the layers, without any other limitation.
[0045] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A composite material roller forming method, characterized in that: include: After impregnating a number of bundles of carbon fibers with resin glue, they are wound on a mold. During the winding process, the carbon fiber winding tension, longitudinal winding angle, thickness of a single continuous longitudinal winding layer and content of resin glue are all controlled within a preset range, and the thickness ratio of the longitudinal / circumferential layers is a preset value to form a roller body; A high temperature resistant film is provided on the outside of the roller body; Heating and curing the roller body until the curing degree of the roller body reaches a preset range; Separating the cured roller body from the high temperature resistant film, and separating the cured roller body from the mold to form a composite material roller body; Connecting structures are arranged at both ends of the composite material roller body; The composite material roller body and the connection structure are subjected to surface treatment and dynamic balancing treatment until the surface roughness and circumferential runout detection of the composite material roller body and the connection structure meet preset requirements.
2. The composite material roller forming method according to claim 1, characterized in that: The carbon fiber winding tension is 70~100N / bundle; the longitudinal winding angle is 10~15°; the thickness of the single continuous longitudinal winding layer does not exceed 4mm; the resin glue content is 10%-20%; and the thickness ratio of the longitudinal / circumferential plies is 20 / 1.
3. The composite material roller forming method according to claim 1, characterized in that: The curing degree of the roller body reaches more than 90%.
4. The composite material roller forming method according to claim 1, characterized in that: The method of setting the connection structure at both ends of the composite material roller body is: Cutting both ends of the composite material roll; Ends are pressed into the composite material roller at both ends; Holes are drilled around the contact area between the end head and the composite material roller body, and fasteners are arranged in the holes to fix the end head and the composite material roller body.
5. The composite material roller forming method according to claim 4, characterized in that: Also includes: Before the two ends of the composite material roller body are respectively pressed into the end heads, the contact area between the composite material roller body and the end heads is sandblasted and AB mixed glue is applied.
6. The composite material roller forming method according to claim 1, characterized in that: The circular runout detection requirement is: when the composite material roller rotates at 360 r / min, the circular runout is ≤0.03 mm.
7. The composite material roller forming method according to claim 1, characterized in that: Also includes: A composite material covering layer is arranged on the outer side of the composite material roller body.
8. The composite material roller forming method according to claim 7, characterized in that: The method for setting a composite material coating layer on the outside of a composite material roller body is as follows: using an industrial acetone solution to clean the surface of the composite material roller body, evenly applying a resin glue liquid on the surface of the composite material roller body, and evenly wrapping a carbon fiber prepreg tape cut according to a designed size onto the surface of the composite material roller body coated with the resin glue liquid, and forming a composite material coating layer after curing.
9. The composite material roller forming method according to claim 1, characterized in that: The method for arranging the high temperature resistant film on the outer side of the roller body is as follows: firstly winding the high temperature resistant polytetrafluoroethylene tape on the outer side of the roller body, and then winding the glass fiber hoop dry yarn.
10. A roller for a lithium-ion battery roller press, characterized in that: include: An end head (1), a composite material roller body (2), a fastener (3) and a composite material coating layer (4); the end head (1) is pressed into both ends of the composite material roller body (2), a contact area between the end head (1) and the composite material roller body (2) is provided with drill holes around the periphery, and the fastener (3) is screwed into the drill holes; and the composite material coating layer (4) covers the outer periphery of the composite material roller body (2).