Anti-slip wear-resistant fully-dyed floor mat and production process thereof
By using functional composite powder in anti-slip and wear-resistant floor mats, the problems of insufficient antibacterial properties and durability are solved, achieving highly efficient antibacterial and wear-resistant performance of the floor mats and improving their stability and safety in use.
Patent Information
- Application Number
- CN202410974040.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing anti-slip and wear-resistant floor mats have shortcomings in terms of antibacterial properties and durability, especially when used in sports venues. Silver ion antibacterial agents have poor durability and high cost, while the antibacterial effect of nanofillers is unstable.
Using self-made functional composite powder, lanthanum-doped carbon dots are generated through hydrothermal reaction and combined with zinc oxide particles to prepare antibacterial powder. Furthermore, by modifying antioxidants, its dispersibility and compatibility in styrene-butadiene rubber matrix are enhanced to form a stable composite structure, thereby improving antibacterial properties and durability.
It improves the antibacterial properties and durability of the floor mat, enhances the mechanical properties and aging resistance of the surface material, and reduces the risk of migration of antibacterial agents.
Smart Images

Figure BDA0004954031720000101 
Figure BDA0004954031720000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of floor mats, and in particular relates to a non-slip and wear-resistant fully dyed floor mat and a production process thereof. Background Art
[0002] Rubber floor mats are made of natural rubber, synthetic rubber or other polymer materials, while anti-slip and wear-resistant floor mats are specially used to enhance the anti-slip performance and durability of the floor. They are usually used in homes, commercial and industrial places.
[0003] Common anti-skid and wear-resistant floor mat materials include EPDM rubber and styrene-butadiene rubber, which are highly elastic, anti-skid and wear-resistant, sound-absorbing and shock-absorbing, environmentally friendly and pollution-free. They are comfortable to the feet and are suitable for gyms, playgrounds, parks and other sports venues. Especially in sports venues such as gyms, the sweat of athletes will flow onto the floor mats, and the rubber material itself has no antibacterial function. The rubber floor mats with slightly better antibacterial effects add silver ion antibacterial agents to the wear-resistant layer on the surface, but the durability is poor and the cost of use is high. Some also add nano-fillers to the surface layer, which have higher antibacterial stability and durability, but the antibacterial effect is often not as good as the silver ion antibacterial agent. Therefore, it is necessary to improve the durability and antibacterial properties of the antibacterial materials in the rubber floor mats at the same time. Summary of the invention
[0004] The purpose of the present invention is to provide a non-slip and wear-resistant fully dyed floor mat, and the antibacterial property and durability of the floor mat are improved by homemade functional composite powder; the second purpose of the present invention is to provide a production process of a non-slip and wear-resistant fully dyed floor mat.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A non-slip and wear-resistant fully dyed floor mat comprises a base layer formed by bonding and curing styrene-butadiene rubber particles, and a composite surface layer on the base layer.
[0007] A production process of a non-slip and wear-resistant fully dyed floor mat, comprising the following steps:
[0008] Step 1: Add styrene-butadiene rubber particles, white carbon black, calcium carbonate powder, phosphorus flame retardant, functional composite powder, glass fiber, ultraviolet absorber, antioxidant, foaming agent, accelerator, sulfur, stearic acid, liquid paraffin and color powder into an internal mixer, mix at 150-160° C. for 2-3 minutes, then transfer to a flat vulcanizer, press vulcanize at 160-180° C. and 12-14 MPa for 20-25 minutes, cut and shape to obtain a surface layer with a thickness of 3-5 mm;
[0009] Step 2: Evenly mix the styrene-butadiene rubber particles and the polyurethane adhesive in a mass ratio of 7-8:1 to obtain a base mixture, spread the base mixture evenly in a mold and adhere the surface layer to the surface, cure and mold at 160-180°C and a pressure of 6-8MPa, and demold to obtain a non-slip and wear-resistant fully dyed floor mat.
[0010] Furthermore, the mass ratio of styrene-butadiene rubber particles, white carbon black, calcium carbonate powder, phosphorus flame retardant, functional composite powder, glass fiber, ultraviolet absorber, antioxidant, foaming agent, accelerator, sulfur, stearic acid, liquid paraffin and color powder is 10-12: 3-4: 3-4: 1-1.5: 1-1.2: 0.3-0.5: 0.3-0.5: 0.3-0.5: 0.8-1.3: 0.5-1: 0.15-0.16: 0.13-0.15: 3-4: 1.5-2.5.
[0011] Furthermore, the phosphorus-based flame retardant is any one of n-butyl bis(hydroxypropyl)phosphine oxide and tri(hydroxypropyl)phosphine oxide.
[0012] Furthermore, the length of the glass fiber is 2-3 mm.
[0013] Furthermore, the ultraviolet absorber is any one of 2,4-dihydroxybenzophenone and 2-hydroxy-4-n-octyloxybenzophenone.
[0014] Furthermore, the antioxidant is any one of antioxidant 168 , antioxidant 702 and antioxidant 703 .
[0015] Furthermore, the foaming agent is azodicarbonamide.
[0016] Furthermore, the accelerator is any one of accelerator M, accelerator DM and accelerator MZ.
[0017] Furthermore, the functional composite powder is prepared by the following steps:
[0018] Step 1: Add lanthanum chloride, ethylenediamine and deionized water into a reactor, stir for 3-5 minutes at 20-25°C and 200-300r / min, then add lysine and zinc oxide precursor, continue stirring for 10-20 minutes, ultrasonically disperse for 5-10 minutes, and keep warm for reaction at 200-220°C for 12-16 hours. Through a hydrothermal reaction, ethylenediamine and lysine are used as carbon sources to generate carbon dots with carboxyl and amino groups, and lanthanum chloride is converted into lanthanum oxide. These lanthanum-doped carbon dots will grow with zinc oxide particles as templates. The reaction solution is naturally cooled, filtered through a 0.45μm filter, and the filtrate is collected and freeze-dried to obtain an antibacterial powder;
[0019] Step 2: Add N-phenyl-p-phenylenediamine and toluene to the reactor, stir until the N-phenyl-p-phenylenediamine is dissolved, add 3-isocyanatepropyltrimethoxysilane and dibutyltin dilaurate as a catalyst to the reactor under nitrogen protection, stir and react for 3-3.5 hours at 50-55° C. and 800-1000 r / min, remove toluene by rotary evaporation, and extract the remaining product with anhydrous ethanol to remove unreacted monomers to obtain a modified antioxidant;
[0020] Step 3: Add the antibacterial agent powder, modified antioxidant and 90% ethanol aqueous solution into the reactor, stir at 200-300 r / min for 3-5 min, then ultrasonically disperse for 5-10 min, adjust the pH value to 4-4.5 with acetic acid, stir the reaction at 50-60°C for 10-12 h, centrifuge and filter, wash the precipitate with anhydrous ethanol for 3-5 times, and vacuum dry to obtain a functional composite powder.
[0021] Furthermore, in step 1, the dosage ratio of lanthanum chloride, ethylenediamine, deionized water, lysine and zinc oxide precursor is 1.2-1.25 g: 1 mL: 400-500 mL: 4.5-5 g: 12-13.5 g.
[0022] Furthermore, in step 2, the usage ratio of N-phenyl-p-phenylenediamine, toluene, 3-isocyanatepropyltrimethoxysilane and dibutyltin dilaurate is 4.4-4.5 g: 60-65 mL: 3.8-4 g: 0.1 g.
[0023] Furthermore, in step 3, the dosage ratio of the antibacterial agent powder, the modified antioxidant and the ethanol aqueous solution is 10g:1.5-1.8g:350-400mL.
[0024] Furthermore, in step 1, the zinc oxide precursor is prepared by the following steps:
[0025] Hexadecyltrimethylammonium bromide, zinc nitrate hexahydrate and deionized water are added into a reaction kettle, stirred at 200-500r / min for 20-30min, then a sodium hydroxide solution with a molar concentration of 1mol / L is added into the reaction kettle, then stirred at 20-25℃ for 100-120min, then kept warm at 180-185℃ for 30-40min, cooled naturally, centrifuged and filtered, the precipitate is washed with anhydrous ethanol for 3-5 times, vacuum dried at 50-60℃, ground and crushed to obtain a zinc oxide precursor.
[0026] Furthermore, the usage ratio of hexadecyltrimethylammonium bromide, zinc nitrate hexahydrate, deionized water and sodium hydroxide solution is 2.5-2.65 g: 19-20 g: 80-100 mL: 140-150 mL.
[0027] Beneficial effects of the present invention:
[0028] The surface layer of the anti-skid and wear-resistant fully dyed floor mat of the present invention is added with a functional composite material during the production process. The functional composite material has good antibacterial and anti-aging effects, which helps to increase the antibacterial performance and durability of the fully dyed floor mat product.
[0029] In the preparation process of the functional composite powder of the present invention, a zinc oxide precursor is used as the main material. The zinc oxide precursor is generated by reacting zinc nitrate and sodium hydroxide. Through a hydrothermal reaction, ethylenediamine and lysine are used as carbon sources to generate carbon dots that inherit carboxyl and amino groups. Lanthanum chloride is converted into lanthanum oxide. These lanthanum-doped carbon dots grow with zinc oxide particles as templates to form a stable composite structure, thereby preparing an antibacterial agent powder. During the hydrothermal reaction, the zinc oxide precursor forms zinc oxide with a nanometer particle size, which can play a good antibacterial role. After being compounded with lanthanum oxide, a synergistic effect is played to enhance the photocatalytic activity of zinc oxide and improve the bactericidal effect. At the same time, the carbon dots have good antibacterial properties. After being modified with lysine, the amino groups on the surface of the carbon dots can be increased, and electrostatic effects are generated with the negative charges on the surface of bacteria, destroying the bacterial cell structure to dissolve and kill them, further enhancing the bactericidal activity of the functional composite powder.
[0030] The isocyanate group in 3-isocyanatepropyltrimethoxysilane reacts with the amino group on the antioxidant N-phenyl-p-phenylenediamine to prepare a modified antioxidant, which is hydrolyzed under weakly acidic conditions to produce a silanol group. The inherited carboxyl group and the silanol group in the antibacterial agent powder are in situ bonded to finally prepare a functional composite powder; the modified antioxidant is coated with the antibacterial agent powder particles by in situ bonding, which helps to increase the dispersibility and compatibility of the antibacterial agent powder in the styrene-butadiene rubber matrix, helps to further improve the mechanical properties of the surface material, and can reduce the migration of N-phenyl-p-phenylenediamine during use, which helps to increase the aging resistance and stability of the surface material. DETAILED DESCRIPTION
[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1: This example provides a non-slip and wear-resistant fully dyed floor mat, which is prepared by the following production process:
[0033] Step 1: Add 25 kg of hexadecyltrimethylammonium bromide, 190 kg of zinc nitrate hexahydrate and 800 L of deionized water into a reactor, stir at 200 r / min for 20 min, then add 1400 L of 1 mol / L sodium hydroxide solution into the reactor, then stir at 20° C. for 100 min, then keep warm at 180° C. for 30 min, cool naturally, centrifuge and filter, wash the precipitate with anhydrous ethanol 3 times, vacuum dry at 50° C., grind and crush to obtain a zinc oxide precursor.
[0034] Step 2: Add 1.2 kg of lanthanum chloride, 1 L of ethylenediamine and 400 L of deionized water into the reactor, stir for 3 min at 20 ° C and 200 r / min, then add 4.5 kg of lysine and 12 kg of zinc oxide precursor, continue stirring for 10 min, ultrasonically disperse for 5 min, and keep warm at 200 ° C for 12 h. Through hydrothermal reaction, ethylenediamine and lysine are used as carbon sources to generate carbon dots inheriting carboxyl and amino groups. These carbon dots will grow with zinc oxide particles as templates. The reaction solution is naturally cooled, filtered through a 0.45 μm filter, the filtrate is collected and freeze-dried to obtain an antibacterial powder.
[0035] Step 3: Add 4.4 kg of N-phenyl-p-phenylenediamine and 60 L of toluene to the reactor, stir until the N-phenyl-p-phenylenediamine is dissolved, then add 3.8 kg of 3-isocyanatepropyltrimethoxysilane and 0.1 kg of dibutyltin dilaurate as a catalyst to the reactor under nitrogen protection, stir and react at 50°C and 800 r / min for 3 hours, remove toluene by rotary evaporation, and extract the remaining product with anhydrous ethanol to remove unreacted monomers to obtain a modified antioxidant.
[0036] Step 4: Add 10 kg of antibacterial agent powder, 1.5 kg of modified antioxidant and 350 L of 90% ethanol aqueous solution into the reactor, stir at 200 r / min for 3 min, then ultrasonically disperse for 5 min, adjust the pH value to 4 with acetic acid, stir the reaction at 50 ° C for 10 h, centrifuge and filter, wash the precipitate with anhydrous ethanol 3 times, and vacuum dry to obtain a functional composite powder.
[0037] Step 5: Add 10kg of styrene-butadiene rubber particles, 3kg of white carbon black, 3kg of calcium carbonate powder, 1kg of n-butyl bis(hydroxypropyl)phosphine oxide, 1kg of functional composite powder, 0.3kg of glass fiber with a length of 2-3mm, 0.3kg of 2,4-dihydroxybenzophenone, 0.3kg of antioxidant 168, 0.8kg of azodicarbonamide as a foaming agent, 0.5kg of accelerator M, 0.15kg of sulfur, 0.13kg of stearic acid, 3kg of liquid paraffin and 1.5kg of color powder into an internal mixer, mix at 150°C for 2min, then transfer to a flat vulcanizer, pressurize and vulcanize at 160°C and a pressure of 12MPa for 20min, cut and shape to obtain a surface layer with a thickness of 3mm.
[0038] Step six: Evenly mix the styrene-butadiene rubber particles and the polyurethane adhesive in a mass ratio of 7:1 to obtain a base mixture, spread the base mixture evenly in a mold and adhere the surface layer to the surface, cure and shape it at 160°C and a pressure of 6MPa, and demold to obtain a non-slip and wear-resistant fully dyed floor mat.
[0039] Example 2: This example provides a non-slip and wear-resistant fully dyed floor mat, which is prepared by the following production process:
[0040] Step 1: Add 25.8 kg of hexadecyltrimethylammonium bromide, 195 kg of zinc nitrate hexahydrate and 900 L of deionized water into a reactor, stir at 350 r / min for 25 min, then add 1450 L of 1 mol / L sodium hydroxide solution into the reactor, then stir at 22 ° C for 110 min, then keep warm at 182 ° C for 35 min, cool naturally, centrifuge and filter, wash the precipitate with anhydrous ethanol 4 times, vacuum dry at 55 ° C, grind and crush to obtain a zinc oxide precursor.
[0041] Step 2: Add 1.23 kg of lanthanum chloride, 1 L of ethylenediamine and 450 L of deionized water into the reactor, stir for 4 min at 22 ° C and 250 r / min, then add 4.8 kg of lysine and 12.8 kg of zinc oxide precursor, continue stirring for 15 min, ultrasonically disperse for 8 min, and keep warm at 210 ° C for 14 h. Through hydrothermal reaction, ethylenediamine and lysine are used as carbon sources to generate carbon dots inheriting carboxyl and amino groups. These carbon dots will grow with zinc oxide particles as templates. The reaction solution is naturally cooled, filtered through a 0.45 μm filter, the filtrate is collected and freeze-dried to obtain an antibacterial powder.
[0042] Step 3: Add 4.45 kg of N-phenyl-p-phenylenediamine and 62.5 L of toluene to the reactor, stir until the N-phenyl-p-phenylenediamine is dissolved, then add 3.9 kg of 3-isocyanatepropyltrimethoxysilane and 0.1 kg of dibutyltin dilaurate as a catalyst to the reactor under nitrogen protection, stir and react at 52 ° C and 900 r / min for 3.2 hours, remove toluene by rotary evaporation, and extract the remaining product with anhydrous ethanol to remove unreacted monomers to obtain a modified antioxidant.
[0043] Step 4: Add 10 kg of antibacterial agent powder, 1.65 kg of modified antioxidant and 380 L of 90% ethanol aqueous solution into the reactor, stir at 250 r / min for 4 min, then ultrasonically disperse for 8 min, adjust the pH value to 4.2 with acetic acid, stir the reaction at 55 ° C for 11 h, centrifuge and filter, wash the precipitate with anhydrous ethanol 4 times, and vacuum dry to obtain a functional composite powder.
[0044] Step 5: 11kg of styrene-butadiene rubber particles, 3.5kg of white carbon black, 3.5kg of calcium carbonate powder, 1.25kg of n-butyl bis(hydroxypropyl)phosphine oxide, 1.1kg of functional composite powder, 0.4kg of glass fiber with a length of 2-3mm, 0.4kg of 2,4-dihydroxybenzophenone, 0.4kg of antioxidant 702, 1kg of azodicarbonamide as a foaming agent, 0.8kg of accelerator DM, 0.155kg of sulfur, 0.14kg of stearic acid, 3.5kg of liquid paraffin and 2kg of color powder are added to an internal mixer, mixed at 155°C for 2.5min, and then transferred to a flat vulcanizer, pressurized and vulcanized at 170°C and a pressure of 13MPa for 23min, cut and formed to obtain a surface layer with a thickness of 4mm.
[0045] Step six: Evenly mix the styrene-butadiene rubber particles and the polyurethane adhesive in a mass ratio of 15:2 to obtain a base mixture, spread the base mixture evenly in a mold and adhere the surface layer to the surface, cure and shape it at 170°C and a pressure of 7MPa, and demold to obtain a non-slip and wear-resistant fully dyed floor mat.
[0046] Example 3: This example provides a non-slip and wear-resistant fully dyed floor mat, which is prepared by the following production process:
[0047] Step 1: Add 26.5 kg of hexadecyltrimethylammonium bromide, 200 kg of zinc nitrate hexahydrate and 1000 L of deionized water into a reactor, stir at 500 r / min for 30 min, then add 1500 L of 1 mol / L sodium hydroxide solution into the reactor, then stir at 25° C. for 120 min, then keep warm at 185° C. for 40 min, cool naturally, centrifuge and filter, wash the precipitate with anhydrous ethanol 5 times, vacuum dry at 60° C., grind and crush to obtain a zinc oxide precursor.
[0048] Step 2: Add 1.25kg of lanthanum chloride, 1L of ethylenediamine and 500L of deionized water into the reactor, stir for 5min at 25°C and 300r / min, then add 5kg of lysine and 13.5kg of zinc oxide precursor, continue stirring for 20min, ultrasonically disperse for 10min, and keep warm at 220°C for 16h. Through hydrothermal reaction, ethylenediamine and lysine are used as carbon sources to generate carbon dots inheriting carboxyl and amino groups. These carbon dots will grow with zinc oxide particles as templates. The reaction solution is naturally cooled, filtered through a 0.45μm filter, the filtrate is collected and freeze-dried to obtain an antibacterial powder.
[0049] Step 3: Add 4.5 kg of N-phenyl-p-phenylenediamine and 65 L of toluene to the reactor, stir until the N-phenyl-p-phenylenediamine is dissolved, then add 4 kg of 3-isocyanatepropyltrimethoxysilane and 0.1 kg of dibutyltin dilaurate as a catalyst to the reactor under nitrogen protection, stir and react at 55 ° C and 1000 r / min for 3.5 hours, remove toluene by rotary evaporation, and extract the remaining product with anhydrous ethanol to remove unreacted monomers to obtain a modified antioxidant.
[0050] Step 4: Add 10 kg of antibacterial agent powder, 1.8 kg of modified antioxidant and 400 L of 90% ethanol aqueous solution into the reactor, stir at 300 r / min for 5 min, then ultrasonically disperse for 10 min, adjust the pH value to 4.5 with acetic acid, stir the reaction at 60 ° C for 12 h, centrifuge and filter, wash the precipitate with anhydrous ethanol 5 times, and vacuum dry to obtain a functional composite powder.
[0051] Step 5: Add 12kg of styrene-butadiene rubber particles, 4kg of white carbon black, 4kg of calcium carbonate powder, 1.5kg of trihydroxypropylphosphine oxide, 1.2kg of functional composite powder, 0.5kg of glass fiber with a length of 2-3mm, 0.5kg of 2-hydroxy-4-n-octyloxybenzophenone, 0.5kg of antioxidant 703, 0.8-1.3kg of azodicarbonamide as a foaming agent, 1kg of accelerator MZ, 0.16kg of sulfur, 0.13-0.15kg of stearic acid, 4kg of liquid paraffin and 2.5kg of color powder into an internal mixer, mix at 160°C for 3min, then transfer to a flat vulcanizer, pressurize and vulcanize at 180°C and a pressure of 14MPa for 25min, cut and shape to obtain a surface layer with a thickness of 5mm.
[0052] Step six: Evenly mix the styrene-butadiene rubber particles and the polyurethane adhesive in a mass ratio of 8:1 to obtain a base mixture, spread the base mixture evenly in a mold and adhere the surface layer to the surface, cure and shape it at 180°C and a pressure of 8MPa, and demold it to obtain a non-slip and wear-resistant fully dyed floor mat.
[0053] Comparative Example 1: Based on Example 3, the functional composite powder was replaced with 1 kg of antibacterial agent powder and 0.2 kg of N-phenyl-p-phenylenediamine, and the other steps remained unchanged to prepare a surface layer.
[0054] Comparative Example 2: Based on Example 3, the functional composite powder was replaced with 1 kg of zinc oxide powder and 0.2 kg of N-phenyl-p-phenylenediamine, and the other steps remained unchanged to prepare a surface layer.
[0055] Comparative Example 3: Based on Example 3, lysine was not added in step 2, and the other steps remained unchanged to prepare a surface layer.
[0056] Comparative Example 4: Based on Example 1, lanthanum chloride was not added in step 2, and the other steps remained unchanged to prepare a surface layer.
[0057] In the embodiments and comparative examples, the styrene-butadiene rubber particles are styrene-butadiene 1502 produced by Jilin Petrochemical; the glass fiber is alkali-free chopped glass fiber purchased from Tai'an Songze Composite Materials Co., Ltd.; the three antioxidants are purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd.; the liquid paraffin is purchased from Shandong Lifeng Chemical Co., Ltd., model D80; and the toner is conventional commercially available iron black.
[0058] Performance tests were conducted on Examples 1 to 3 and Comparative Examples 1 to 4. Different surface layer materials were mixed and pressurized in the same manner as in the steps to prepare different samples with reference to the corresponding test standards:
[0059] The tensile properties of different samples were tested with reference to GB / T 528-2009 at a tensile rate of 50 mm / min. The tear properties of different samples were tested with reference to GB / T529-2008. The abrasion resistance of different samples was tested with a rotary roller abrader with reference to ISO 4649:2017, and the volume loss was recorded. The samples were aged at 150°C for 168 hours with reference to GB / T 3512-2001, and the tensile and tear properties of different samples were tested again.
[0060] Test the antibacterial performance: prepare different materials into specimens with specifications of 50mm×50mm×5mm, place the specimens in an autoclave, sterilize at 121℃, 103kPa for 15min, and set aside; refer to the test method in QB / T 2591-2003, the specimens are equivalent to the antibacterial plastic samples in the standard, Staphylococcus aureus (ATCC 6538), Klebsiella pneumoniae (ATCC 4352) and Escherichia coli (ATCC 11229) are selected as test bacteria, record the data and finally calculate the antibacterial rate (%) of different specimens.
[0061] The test results are shown in Table 1:
[0062] Table 1
[0063]
[0064]
[0065] Staphylococcus aureus is a Gram-positive bacterium, Klebsiella pneumoniae and Escherichia coli are Gram-negative bacteria. It can be seen from Table 1 that the surface materials in Examples 1 to 3 have good antibacterial effects on both types of bacteria. It can be seen from the combination of Comparative Examples 1 and 2 that zinc oxide plays a major antibacterial role and can increase wear resistance. It can be seen from Comparative Example 3 that the addition of lysine during the preparation process helps to improve the antibacterial effect on Gram-negative bacteria, and it can be seen from Comparative Example 4 that the doping of lanthanum improves the antibacterial effect.
[0066] In terms of mechanical properties, zinc oxide in the functional composite powder can improve the tensile strength of the surface material, while the addition of lysine and in-situ bonded N-phenyl-p-phenylenediamine can also improve the tensile strength of the surface material, especially the anti-aging performance of the surface material.
[0067] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0068] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A non-slip and wear-resistant fully dyed floor mat, comprising a base layer and a surface layer, characterized in that: The surface layer comprises the following raw materials by mass: 10-12 parts of styrene-butadiene rubber particles, 3-4 parts of white carbon black, 3-4 parts of calcium carbonate powder, 1-1.5 parts of phosphorus flame retardant, 1-1.2 parts of functional composite powder, 0.3-0.5 parts of glass fiber, 0.3-0.5 parts of ultraviolet absorber, 0.3-0.5 parts of antioxidant, 0.8-1.3 parts of azodicarbonamide, 0.5-1 parts of accelerator, 0.15-0.16 parts of sulfur, 0.13-0.15 parts of stearic acid, 3-4 parts of liquid paraffin and 1.5-2.5 parts of color powder; the length of the glass fiber is 2-3 mm; The functional composite powder is prepared by the following steps: The antibacterial agent powder, the modified antioxidant and the 90wt% ethanol aqueous solution are added into the reaction kettle in the dosage ratio of 10g:1.5-1.8g:350-400mL, stirred at 200-300r / min for 3-5min, ultrasonically dispersed for 5-10min, the pH value is adjusted to 4-4.5 with acetic acid, stirred at 50-60℃ for 10-12h, centrifuged, washed and vacuum dried to obtain the functional composite powder.
2. The anti-skid and wear-resistant fully dyed floor mat according to claim 1, characterized in that: The antibacterial powder is prepared by the following steps: Add lanthanum chloride, ethylenediamine and deionized water into a reaction kettle, stir at 20-25°C and 200-300 r / min for 3-5 minutes, then add lysine and zinc oxide precursor and continue stirring for 10-20 minutes, ultrasonically disperse for 5-10 minutes, keep warm at 200-220°C for 12-16 hours, cool naturally, filter with a 0.45 μm filter, collect the filtrate and freeze-dry to obtain an antibacterial agent powder; The dosage ratio of the lanthanum chloride, ethylenediamine, deionized water, lysine and zinc oxide precursor is 1.2-1.25 g: 1 mL: 400-500 mL: 4.5-5 g: 12-13.5 g.
3. The anti-skid and wear-resistant fully dyed floor mat according to claim 1, characterized in that: The modified antioxidant is prepared by the following steps: Add N-phenyl-p-phenylenediamine and toluene to a reaction kettle, stir until the N-phenyl-p-phenylenediamine is dissolved, add 3-isocyanatepropyltrimethoxysilane and dibutyltin dilaurate to the reaction kettle under nitrogen protection, stir and react at 50-55° C. and 800-1000 r / min for 3-3.5 hours, remove toluene by rotary evaporation, extract the remaining product with anhydrous ethanol to remove unreacted monomers, and obtain a modified antioxidant; The dosage ratio of the N-phenyl-p-phenylenediamine, toluene, 3-isocyanatepropyltrimethoxysilane and dibutyltin dilaurate is 4.4-4.5 g: 60-65 mL: 3.8-4 g: 0.1 g.
4. The anti-skid and wear-resistant fully dyed floor mat according to claim 2, characterized in that: The zinc oxide precursor is prepared by the following steps: Add hexadecyltrimethylammonium bromide, zinc nitrate hexahydrate and deionized water into a reaction kettle, stir at 200-500r / min for 20-30min, then add 1mol / L sodium hydroxide solution, stir at 20-25℃ for 100-120min, keep warm at 180-185℃ for 30-40min, cool naturally, centrifuge, wash, vacuum dry, grind and crush to obtain a zinc oxide precursor.
5. The anti-skid and wear-resistant fully dyed floor mat according to claim 4, characterized in that: The dosage ratio of the hexadecyltrimethylammonium bromide, zinc nitrate hexahydrate, deionized water and sodium hydroxide solution is 2.5-2.65 g: 19-20 g: 80-100 mL: 140-150 mL.
6. The anti-skid and wear-resistant fully dyed floor mat according to claim 1, characterized in that: The phosphorus-based flame retardant is any one of n-butyl bis(hydroxypropyl)phosphine oxide and tri(hydroxypropyl)phosphine oxide.
7. The anti-skid and wear-resistant fully dyed floor mat according to claim 1, characterized in that: The ultraviolet absorber is any one of 2,4-dihydroxybenzophenone and 2-hydroxy-4-n-octyloxybenzophenone.
8. The anti-skid and wear-resistant fully dyed floor mat according to claim 1, characterized in that: The antioxidant is any one of antioxidant 168, antioxidant 702 and antioxidant 703.
9. The anti-skid and wear-resistant fully dyed floor mat according to claim 1, characterized in that: The accelerator is any one of accelerator M, accelerator DM and accelerator MZ.
10. The production process of a non-slip and wear-resistant fully dyed floor mat according to claim 1, characterized in that: The steps include: Step 1: Add the raw materials of the surface layer into an internal mixer, mix at 150-160°C for 2-3 minutes, then transfer to a flat vulcanizer, pressurize and vulcanize at 160-180°C and 12-14MPa for 20-25 minutes, cut and shape to obtain a surface layer with a thickness of 3-5mm; Step 2: Evenly mix the styrene-butadiene rubber particles and the polyurethane adhesive in a mass ratio of 7-8:1 to obtain a base mixture, spread the base mixture evenly in a mold and adhere the surface layer to the surface, cure and mold at 160-180°C and 6-8MPa pressure, and demold to obtain a non-slip and wear-resistant fully dyed floor mat.
Citation Information
Patent Citations
Antibacterial property resin composite material and preparation method thereof
CN103059549A
Vibration-absorption, wear-resisting and antibacterial rubber floor mat and preparation method thereof
CN109054190A
Nano silicon dioxide / chitosan hybrid material supported anti-aging agent as well as preparation and application thereof
CN115403680A
Preparation method and application of arginine antibacterial carbon dots
CN115849347A
Carbon dot antibacterial composite material and preparation method of modified asphalt thereof
CN117487370A