Preparation method of thermochromic leather composite material based on waste textiles
The waste textiles are made into thermochromic leather composite materials through needle puncture and hot pressing processes, which solves the problem of recycling and utilization of waste textiles, and realizes the preparation of leather composite materials with efficient resource utilization and excellent performance, suitable for automotive interiors and heating Products such as pads and have temperature display function.
Patent Information
- Application Number
- CN202410982330.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The traditional recycling methods of waste carbon fiber have had a serious impact on the environment, and the failure to effectively utilize waste textile resources has led to waste of resources and an increase in the market demand for carbon fiber.
The needle-punching process is used to make waste carbon fiber and waste polyester fiber into carbon fiber needle-punching felt and polyester non-woven fabric, alternately lay and reinforce, impregnate the thermoplastic polyurethane solution, and 3D printing and thermally discolored ink and heat-pressing to prepare Thermal color-changing leather composite.
Prepare leather composite materials with high softness and excellent conductivity and heat transfer performance to reduce resource waste and reduce costs. They are suitable for automotive interiors and heating pads, and realize the temperature display function through the conductivity of carbon fibers.
Smart Images

Figure CN118906587A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of composite materials, in particular to a method for preparing a thermochromic leather composite material based on waste textiles. Background Art
[0002] The amount of waste textiles continues to increase, and the recycling of waste textiles is particularly important. Most of the waste carbon fiber exists in the form of chopped carbon fiber or waste composite materials. The source of waste chopped carbon fiber is mainly the manufacturing process of composite materials, such as waste and scraps generated in the weaving, weaving and non-woven processes of carbon fiber, which accounts for a large part (up to 40%) of the entire waste carbon fiber recycling. Traditional methods of recycling waste carbon fiber include two physical treatment methods: landfill and incineration, which have a great impact on the environment and cause serious waste of resources.
[0003] Fiber-reinforced composite materials are widely used in many fields due to their high specific strength, large specific modulus, good corrosion resistance, strong designability, and good durability. For example, they have great development advantages in the process application of various components in aerospace and automobiles, and can be used for seat cushions, etc. Therefore, recycling waste carbon fiber for the preparation of fiber-reinforced composite materials, especially automotive interiors or parts, not only reduces resource waste, but also eases the market demand for carbon fiber, which is an urgent research direction. Summary of the invention
[0004] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a method for preparing a thermochromic leather composite material based on waste textiles.
[0005] The technical solution of the present invention to solve the technical problem is to provide a method for preparing a thermochromic leather composite material based on waste textiles, characterized in that the method comprises the following steps:
[0006] Step 1, using waste carbon fiber and waste polyester fiber as raw materials, respectively preparing carbon fiber needle felt and polyester non-woven fabric through a needle punching process; then using carbon fiber needle felt and polyester non-woven fabric as raw materials, first laying the carbon fiber needle felt and polyester non-woven fabric in an alternating manner, and then performing needle punching reinforcement on the whole to prepare a composite material preform with both the upper and lower surface layers being polyester non-woven fabrics;
[0007] Step 2, immersing the preform of step 1 in a thermoplastic polyurethane solution, so that the interior and surface of the preform are filled with the thermoplastic polyurethane solution, to obtain an impregnated preform; then taking out the impregnated preform, drying and evaporating the solvent until the mass of the impregnated preform no longer changes, to obtain a dried preform;
[0008] Step 3: Print the thermochromic ink on the surface of the dried preform by 3D printing; then lay a thermoplastic polyurethane film on the upper and lower surfaces of the printed preform, and heat-press and cure the preform to obtain a thermochromic leather composite material.
[0009] Compared with the prior art, the present invention has the following beneficial effects:
[0010] (1) The present invention uses waste carbon fiber and waste polyester fiber as reinforcing materials and thermoplastic polyurethane as the matrix material, and utilizes a needle punching process and a hot pressing process to give full play to the excellent properties of different reinforcing fibers to produce a leather composite material with high softness, excellent electrical conductivity, heat transfer performance and mechanical properties, which is more suitable for automobile heated seat cushions, desktop heating pads, etc.
[0011] (2) The waste carbon fiber and waste polyester fiber of the present invention are derived from waste textiles and waste scraps, which fully utilize waste resources, reduce resource waste, greatly reduce costs, and are beneficial to achieving high-value utilization of waste textiles.
[0012] (3) The present invention adds carbon fiber to give the leather composite material its corresponding characteristics. On the one hand, the lightweight characteristics of carbon fiber are used to prepare automobile interiors or parts, which can effectively reduce the weight of the vehicle body and make the automobile develop in the direction of lightweight. On the one hand, carbon fiber has high strength and elastic modulus. It can resist strain locally in the surrounding matrix, so that more stress is concentrated on the carbon fiber, thereby playing a reinforcing role. On the other hand, carbon fiber has high conductivity: the surface of the leather composite material is printed with thermochromic ink at different temperatures. By utilizing the conductivity of carbon fiber, after the leather composite material is energized, the pattern is made to show different colors at different temperatures by electric heating. When it is made into a heating pad or other product, the composite material is heated or otherwise changed in temperature when energized, and the corresponding color of the pattern at that temperature is displayed. The temperature of the product can be judged by observing the color of the pattern.
[0013] (4) The present invention adopts three-dimensional needle punching technology to prepare preforms. After needling, needle-punched fibers are continuously introduced into the original multi-layer two-dimensional fiber fabric to achieve the dispersion, rearrangement and fixation of the fiber layers, thereby making the preforms of better quality and better bonding performance, effectively improving the interlayer performance of the leather composite material, improving the interface bonding performance, and reducing the stratification phenomenon.
[0014] (5) The addition of polyester fiber can make the leather composite material highly similar to genuine leather in texture and appearance, while also performing well in terms of waterproofness, anti-fouling, and UV resistance.
[0015] (6) Thermoplastic polyurethane elastomer is used as the matrix material, and the wear resistance and superelastic properties of thermoplastic polyurethane elastomer are fully utilized to improve the performance of leather composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a side super-depth electron microscope image of the carded carbon fiber web of Comparative Example 1 of the present invention;
[0017] Figure 2 This is a super-depth electron microscope image of the tensile fracture of the thermochromic leather composite material prepared in Comparative Example 1 of the present invention;
[0018] Figure 3 This is a side ultra-depth electron microscope image of the carbon fiber needle felt of Example 1 of the present invention;
[0019] Figure 4 This is a super-depth electron microscopy image of the tensile fracture of the thermochromic leather composite material prepared in Example 1 of the present invention;
[0020] Figure 5 A bar graph showing the tensile strength of the thermochromic leather composite material prepared in Examples 1 to 3 of the present invention;
[0021] Figure 6 A bar graph showing the elongation at break of the thermochromic leather composite material prepared in Examples 1 to 3 of the present invention;
[0022] Figure 7 A bar graph showing the tensile strength of the thermochromic leather composite material prepared in Examples 4 to 6 of the present invention;
[0023] Figure 8 A bar graph showing the elongation at break of the thermochromic leather composite material prepared in Examples 4 to 6 of the present invention;
[0024] Fig. 9 This is a diagram of the conductive heat transfer temperature distribution of the thermochromic leather composite material prepared in Example 6 of the present invention;
[0025] Fig.10 This is a graph showing the color change of the thermochromic leather composite material prepared in Example 6 of the present invention as the temperature changes. DETAILED DESCRIPTION
[0026] The specific embodiments of the present invention are given below. The specific embodiments are only used to further illustrate the present invention in detail and do not limit the protection scope of the claims of the present invention.
[0027] The present invention provides a method for preparing a thermochromic leather composite material based on waste textiles (hereinafter referred to as the method), characterized in that the method comprises the following steps:
[0028] Step 1, using waste carbon fiber and waste polyester fiber as raw materials, respectively preparing carbon fiber needle felt and polyester non-woven fabric through a needle punching process; then using carbon fiber needle felt and polyester non-woven fabric as raw materials, first laying the carbon fiber needle felt and polyester non-woven fabric in an alternating manner, and then performing needle punching reinforcement on the whole to prepare a composite material preform (hereinafter referred to as preform) in which both the upper surface layer and the lower surface layer are polyester non-woven fabrics;
[0029] Preferably, in step 1, the needling process is: opening, carding, web laying and needling reinforcement in sequence; the needling reinforcement is preceded by pre-needling and main needling in sequence;
[0030] The preparation of carbon fiber needle-punched felt and polyester non-woven fabric is specifically as follows: first, waste chopped carbon fiber and waste polyester fiber are opened respectively; then, the opened fibers are combed separately so that the combed single fibers are interlaced with each other, and a carbon fiber web and a polyester fiber web are formed respectively after the combing process is completed; then, the fiber webs are stacked separately in a cross-laying manner, and then, they are respectively sent to a needle-punching machine for pre-needling and main needling to form carbon fiber needle-punched felt and polyester non-woven fabric respectively.
[0031] Preferably, in step 1, the needle punching reinforcement process is: the needle punching density is 8 to 60 needles / cm 2 The pre-acupuncture depth is 11-16 mm, and the main acupuncture depth is 6-9 mm.
[0032] Preferably, in step 1, the weight of the polyester nonwoven fabric is 30 to 120 g / m 2 (Preferably 30 to 80 g / m 2 , more preferably 40g / m 2 ); in the thermochromic leather composite material, the volume content of carbon fibers (the volume content of fiber is the percentage of the volume of fiber in the fiber-reinforced composite material to the volume of the composite material) is 4 to 25% (preferably 6 to 12%).
[0033] Step 2, immersing the preform of step 1 in a thermoplastic polyurethane solution, so that the interior and surface of the preform are filled with the thermoplastic polyurethane solution, to obtain an impregnated preform; then taking out the impregnated preform, drying and evaporating the solvent until the mass of the impregnated preform no longer changes, to obtain a dried preform;
[0034] Preferably, in step 2, the impregnation process is: the impregnation temperature is room temperature, and the time is 10 to 30 minutes (preferably 20 to 30 minutes).
[0035] Preferably, in step 2, the mass fraction of the thermoplastic polyurethane solution is 8 to 14 wt %.
[0036] Preferably, in step 2, the preparation of the thermoplastic polyurethane solution is: dissolving the TPU elastomer in a solvent, and obtaining the thermoplastic polyurethane solution after degassing;
[0037] The dissolution process is: adding the TPU elastomer into a solvent, stirring at a temperature of 50 to 80° C. and a speed of 100 to 400 r / min for 2.5 to 5 hours to completely dissolve; the solvent is DMF, acetone, cyclohexanone, butanone, toluene, ethyl acetate or tetrahydrofuran;
[0038] The degassing process is: degassing in a vacuum oven at a temperature of 15 to 35° C. for 15 to 40 minutes (preferably 20 to 30 minutes).
[0039] Preferably, in step 2, the drying process is: placing in an environment with a temperature of 50 to 90° C. (preferably 60 to 80° C.) for 3 to 12 hours to volatilize the solvent until the mass of the preform after impregnation no longer changes.
[0040] Step 3: Print the thermochromic ink on the surface of the dried preform by 3D printing; then lay a thermoplastic polyurethane film on the upper and lower surfaces of the printed preform, place it in a mold, and heat-press and cure it to obtain a thermochromic leather composite material (referred to as leather composite material).
[0041] Preferably, in step 3, the 3D printing process is: placing the dried preform on a substrate (i.e., a printing bed or a building platform of a 3D printing instrument), adding thermochromic ink into a nozzle of the 3D printing instrument, and printing an arbitrary pattern on the surface of the dried preform;
[0042] Preferably, in step 3, the 3D printing process parameters are: printing speed of 10 to 60 mm / s, printing height of 0.5 to 3 mm, number of printing layers of 1 to 8 layers, nozzle temperature of room temperature, and substrate temperature of 30 to 80°C.
[0043] Preferably, in step 3, the preparation process of the thermoplastic polyurethane film is: slowly pouring the thermoplastic polyurethane solution of step 2 onto a release paper or into a mold that is easy to peel off, then using a scraper to evenly apply the thermoplastic polyurethane solution, and then drying to fully volatilize the solvent, and then forming to obtain the thermoplastic polyurethane film;
[0044] The drying process is: drying in an environment of 50-90° C. (preferably 60-80° C.) for 20-80 minutes (preferably 40-50 minutes).
[0045] Preferably, in step 3, the hot pressing curing process is carried out in a hot press, the hot pressing pressure is 3 to 10 MPa (preferably 5 to 7 MPa), the hot pressing temperature is 100 to 200° C. (preferably 140 to 165° C.), and the hot pressing time is 10 to 45 min (preferably 25 to 40 min).
[0046] Performance test: According to the test standard, the thermochromic leather composite material was cut into a dumbbell shape for tensile test. The thermal conductivity of the leather composite material was tested using a TC3000E thermal conductivity meter. The heat transfer performance of the leather composite material was tested by connecting the positive and negative electrodes and applying power to it, and then photographing it with an infrared thermal imager.
[0047] Example 1
[0048] (1) Using waste carbon fiber and waste polyester fiber as raw materials, respectively preparing carbon fiber needle felt and polyester non-woven fabric through a needle punching process; then using carbon fiber needle felt and polyester non-woven fabric as raw materials, laying the carbon fiber needle felt and polyester non-woven fabric in an alternating manner to form a three-layer structure of polyester non-woven fabric-carbon fiber needle felt-polyester non-woven fabric, and then reinforcing the whole by needle punching to prepare a three-layer composite material preform in which the upper surface layer and the lower surface layer are both polyester non-woven fabrics and the middle layer is carbon fiber needle felt;
[0049] The acupuncture density is 15 needles / cm 2 , the pre-needling depth is 11mm, the main needling depth is 9mm, the carbon fiber volume content is 12%, and the weight of the polyester non-woven fabric is 40g / m 2 ;
[0050] (2) adding a TPU elastomer to DMF, stirring at 60°C and 200 r / min for 3 h, taking it out and degassing it in a vacuum oven at 25°C for 30 min to obtain a 12 wt% thermoplastic polyurethane solution; at room temperature, immersing the preform in the thermoplastic polyurethane solution for 20 min so that the interior and surface of the preform are filled with the thermoplastic polyurethane solution to obtain an impregnated preform; then taking out the impregnated preform and placing it in a 60°C environment for 8 h to completely volatilize the DMF to obtain a dried preform;
[0051] (3) placing the dried preform on a substrate, adding thermochromic ink into the nozzle of a 3D printing instrument, and printing the thermochromic ink on the surface of the dried preform by 3D printing technology, with a printing speed of 40 mm / s, a printing height of 1 mm, a printing layer number of 2 layers, a nozzle temperature of room temperature, and a substrate temperature of 50°C; then laying a thermoplastic polyurethane film on the upper and lower surfaces of the printed preform and placing it in a mold, and then placing the whole into a hot press at a hot pressing pressure of 6 MPa and hot pressing at 140°C for 25 minutes to cure and form, thereby obtaining a thermochromic leather composite material.
[0052] The preparation process of the thermoplastic polyurethane film is as follows: slowly pouring the thermoplastic polyurethane solution of step (2) onto release paper or into a mold that is easy to peel off, then using a scraper to evenly apply the thermoplastic polyurethane solution, then drying in an environment of 60° C. for 60 minutes to fully volatilize the solvent, and obtaining the thermoplastic polyurethane film after molding;
[0053] Comparative Example 1
[0054] Comparative Example 1 is completely the same as Example 1, except that in step (1), the carded carbon fiber web (i.e., not subjected to web laying and needle punching reinforcement) and polyester non-woven fabric are used as raw materials to lay the web to form a three-layer structure of polyester non-woven fabric-carbon fiber web-polyester non-woven fabric. That is, the carded carbon fiber web is used as the middle layer, and needle punching reinforcement is not performed on the whole after laying.
[0055] Comparing the test results of Example 1 with those of Comparative Example 1, Figure 1 and Figure 2 It can be seen that, in the case of no needle punching reinforcement, the internal fibers are less entangled, the connection between the fibers is not tight enough, the strength of the fiber web is low, and the fiber web is relatively loose, so that the prepared leather composite material is delaminated when subjected to the tensile performance test, and the tensile strength of the final leather composite material is affected. Figure 3 and Figure 4 It can be seen that the method of Example 1 is adopted to repeatedly puncture the fiber web through needle punching technology, so that the fibers on the surface of the fiber web and the local inner layer are forced to penetrate into the interior of the fiber web, so that the fluffy carbon fiber web with the same volume content is compressed due to the friction between the fibers, thereby increasing the entanglement between the fibers, strengthening the fiber web, weakening the stratification, enhancing the interface bonding performance of the leather composite material, and improving the mechanical properties of the leather composite material.
[0056] Comparative Example 2
[0057] The difference between Comparative Example 2 and Example 1 is that in step (2), the mass fraction of the thermoplastic polyurethane solution is 20wt%. Preliminary experiments show that the leather composite material prepared using the solution with a mass fraction of 20wt% as raw material has a hard feel and poor softness.
[0058] Comparative Example 3
[0059] The difference between Comparative Example 3 and Example 1 is that in step (2), the mass fraction of the thermoplastic polyurethane solution is 18 wt %. Preliminary experiments show that the leather composite material prepared using the solution with a mass fraction of 18 wt % as the raw material has a hard feel and poor softness.
[0060] Comparative Example 4
[0061] The difference between Comparative Example 4 and Example 1 is that in step (2), the mass fraction of the thermoplastic polyurethane solution is 15 wt %. Preliminary experiments show that the leather composite material prepared using the solution with a mass fraction of 15 wt % as the raw material has a hard feel and poor softness.
[0062] Example 2
[0063] Example 2 is exactly the same as Example 1, except that in step (1), the volume content of carbon fiber is 9%.
[0064] Example 3
[0065] Example 3 is exactly the same as Example 1, except that in step (1), the volume content of carbon fiber is 6%.
[0066] The test results of comparative examples 1-3 are shown in FIG. Figure 5 and Figure 6 It can be seen that without changing the mass fraction of the thermoplastic polyurethane solution, the tensile strength and elongation at break of Example 1 are 31.29 MPa and 4.85%, respectively, the tensile strength and elongation at break of Example 2 are 28.28 MPa and 6.58%, respectively, and the tensile strength and elongation at break of Example 3 are 27.61 MPa and 9.85%, respectively. The tensile strength of Example 2 is slightly lower than that of Example 1, and the elongation at break of Example 2 is only slightly changed compared with that of Example 1. The tensile strength of Example 3 is slightly lower than that of Example 1, and the elongation at break of Example 3 is improved compared with that of Example 1, but the elongation at break is still small. Comparing the feel of the final leather composite material, the softness of Example 2 is improved compared with that of Example 1; the softness of Example 3 is improved compared with that of Example 1. Therefore, the volume content of carbon fiber affects the softness of the leather composite material, and appropriately reducing the volume content of carbon fiber can improve the softness of the leather composite material.
[0067] Example 4
[0068] Example 4 is exactly the same as Example 1, except that in step (2), the mass fraction of the thermoplastic polyurethane solution is 10 wt %.
[0069] Comparing the test results of Example 4 and Example 1, when the volume content of carbon fiber is 12% and the mass fraction of the thermoplastic polyurethane solution is reduced, the tensile strength and elongation at break of Example 4 are 29.73 MPa and 7.43%, respectively. The tensile strength of Example 4 is slightly lower than that of Example 1, and the elongation at break of Example 4 is slightly improved compared with that of Example 1, and the leather composite material feels relatively soft.
[0070] Example 5
[0071] Example 5 is exactly the same as Example 4, except that in step (1), the volume content of carbon fiber is 9%.
[0072] Example 6
[0073] Example 6 is exactly the same as Example 4, except that in step (1), the volume content of carbon fiber is 6%.
[0074] Comparative Example 4-6 test results, by Figure 7 and Figure 8 It can be seen that in Example 5, due to the decrease in the volume content of carbon fiber, the tensile strength of the leather composite material becomes 27.17MPa, and the elongation at break becomes 9.42%, which are smaller than those in Example 4, and the softness of the hand feel does not change much. In order to improve its elongation at break, the mass fraction of the thermoplastic polyurethane solution is further changed. In Example 6, due to the reduction in the volume content of carbon fiber, the tensile strength of the leather composite material becomes 24.35MPa, which is slightly lower than that in Example 4, and the elongation at break increases to 18.44%. Compared with Example 4, the elongation at break is increased by more than double, and the softness of the composite material is improved, and the hand feel is softer. In summary, the reduction in the mass fraction of the thermoplastic polyurethane solution can also improve the softness of the leather composite material.
[0075] The thermal conductivity of the leather composite material of Example 6 is in the range of 0.54 to 0.56 W / (m·K).
[0076] Use an infrared thermal imager to monitor the temperature change and stability of the leather composite material after applying voltage, and judge the conductive heat transfer effect and stability of the leather composite material, such as Fig. 9 As shown in the figure, when different voltages are applied to the sample, the infrared thermal imager is used for testing. The temperature distribution diagram intuitively reflects the surface temperature of the sample and the lowest and highest temperatures of the photographed area. Among them, Figure a and Figure b show that the surface temperature of the sample is 34.1℃ and 48.0℃ when the voltage is small; Figure c and Figure d are based on Figure a and Figure b, and the voltage is increased. At this time, the surface temperature of the sample also gradually increases to 59.2℃ and 76.9℃. Through the analysis of the temperature distribution diagram taken by the infrared thermal imager, the surface temperature of the sample increases with the increase of voltage, showing that the conductive heat transfer effect is good under different voltages and the heat transfer is relatively uniform and stable.
[0077] The temperature of the leather composite material can be judged by the color of the pattern displayed at different temperatures of the leather composite material. Fig.10 It can be seen that when the pattern is obtained using 45°C thermochromic ink, the pattern is blue at room temperature and turns pink in the process of gradually heating to 45°C, and the leather composite material has a good heat transfer effect.
[0078] According to the mechanical properties and softness of the final leather composite material, a preliminary experiment was carried out as shown in Table 1.
[0079] Table 1
[0080]
[0081]
[0082] Table 2
[0083]
[0084] It can be seen from Table 2 that the leather composite material prepared by the present invention can improve its interface stratification after needling, improve the interface bonding performance of the leather composite material, and the leather composite materials prepared at different carbon fiber volume contents have good heat transfer effects.
[0085] Any matters not described in the present invention are applicable to the prior art.
Claims
1. A method for preparing a thermochromic leather composite material based on waste textiles, characterized in that: The method comprises the following steps: Step 1, using waste carbon fiber and waste polyester fiber as raw materials, respectively preparing carbon fiber needle felt and polyester non-woven fabric through a needle punching process; then using carbon fiber needle felt and polyester non-woven fabric as raw materials, first laying the carbon fiber needle felt and polyester non-woven fabric in an alternating manner, and then performing needle punching reinforcement on the whole to prepare a composite material preform with both the upper and lower surface layers being polyester non-woven fabrics; Step 2, immersing the preform of step 1 in a thermoplastic polyurethane solution, so that the interior and surface of the preform are filled with the thermoplastic polyurethane solution, to obtain an impregnated preform; then taking out the impregnated preform, drying and evaporating the solvent until the mass of the impregnated preform no longer changes, to obtain a dried preform; Step 3: Print the thermochromic ink on the surface of the dried preform by 3D printing; then lay a thermoplastic polyurethane film on the upper and lower surfaces of the printed preform, and heat-press and cure the preform to obtain a thermochromic leather composite material.
2. The method for preparing a thermochromic leather composite material based on waste textiles according to claim 1, characterized in that: In step 1, the needle punching process is: the needle punching density is 8 to 60 needles / cm 2 The pre-acupuncture depth is 11-16 mm, and the main acupuncture depth is 6-9 mm.
3. The method for preparing a thermochromic leather composite material based on waste textiles according to claim 1, characterized in that: In step 1, the weight of the polyester nonwoven fabric is 30-120 g / m 2 (Preferably 30 to 80 g / m 2 , more preferably 40g / m 2 ); in the thermochromic leather composite material, the volume content of carbon fibers (the volume content of fiber is the percentage of the volume of fiber in the fiber-reinforced composite material to the volume of the composite material) is 4 to 25% (preferably 6 to 12%).
4. The method for preparing a thermochromic leather composite material based on waste textiles according to claim 1, characterized in that: In step 2, the dipping process is: the dipping temperature is room temperature, and the dipping time is 10 to 30 minutes.
5. The method for preparing a thermochromic leather composite material based on waste textiles according to claim 1, characterized in that: In step 2, the mass fraction of the thermoplastic polyurethane solution is 8-14wt%.
6. The method for preparing a thermochromic leather composite material based on waste textiles according to claim 1, characterized in that: In step 2, the preparation of the thermoplastic polyurethane solution is as follows: dissolving the TPU elastomer in a solvent and degassing to obtain the thermoplastic polyurethane solution; The dissolution process is: adding the TPU elastomer into a solvent, stirring at a temperature of 50 to 80° C. and a speed of 100 to 400 r / min for 2.5 to 5 hours to completely dissolve; the solvent is DMF, acetone, cyclohexanone, butanone, toluene, ethyl acetate or tetrahydrofuran; The degassing process is: degassing in a vacuum oven at a temperature of 15 to 35° C. for 15 to 40 minutes.
7. The method for preparing a thermochromic leather composite material based on waste textiles according to claim 1, characterized in that: In step 2, the drying process is: placing in an environment with a temperature of 50 to 90° C. for 3 to 12 hours.
8. The method for preparing a thermochromic leather composite material based on waste textiles according to claim 1, characterized in that: In step 3, the 3D printing process parameters are: printing speed is 10-60 mm / s, printing height is 0.5-3 mm, number of printing layers is 1-8 layers, nozzle temperature is room temperature, and substrate temperature is 30-80°C.
9. The method for preparing a thermochromic leather composite material based on waste textiles according to claim 1, characterized in that: In step 3, the preparation process of the thermoplastic polyurethane film is: slowly pouring the thermoplastic polyurethane solution of step 2 onto a release paper or into a mold that is easy to peel off, then evenly coating the thermoplastic polyurethane solution with a scraper, and then drying and volatilizing the solvent, and then forming to obtain the thermoplastic polyurethane film; The drying process is: drying in an environment of 50-90°C for 20-80 minutes.
10. The method for preparing a thermochromic leather composite material based on waste textiles according to claim 1, characterized in that: In step 3, the hot pressing curing process is: the hot pressing pressure is 3 to 10 MPa, the hot pressing temperature is 100 to 200° C., and the hot pressing time is 10 to 45 min.
Citation Information
Patent Citations
Preparation method for needle-punched regenerated leather used as surface leather for automobile interior
CN107574677A
Environment-friendly synthetic leather
CN109695160A
Preparation method of 3D needled waste carbon fiber / polyester composite material
CN117285797A