Micro-nano structure preparation method
By using Al2O3 film as a mask, combined with electron beam exposure and lift-off technology, the problem of manufacturing high-deep aspect ratio micro-nano structures in the existing technology is solved, and high-precision, smooth edge preparation of micro-nano structures is achieved, with depth-to-face ratios. It reaches the limit of ICP equipment, has simple process and high etch selection ratio.
Patent Information
- Application Number
- CN202410955542.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to manufacture a high-deep aspect ratio micro-nano structure with smooth side walls up to several microns or even dozens of microns, and the mask edges are not neat and have high process complexity.
Using Al2O3 film as a mask, by spin-coating resist on the sample layer, exposure development, depositing Al2O3 film and carrying out lift-off process, a high-precision and smooth edge Al2O3 mask is formed, and combined with electron beam exposure and ICP plasma. Body etching method realizes the preparation of high-deep and aspect ratio micro-nano structures.
It realizes high-precision and smooth edge manufacturing of micro-nano structures, with a depth-to-face ratio reaching the limit of ICP equipment, a simple process, an etching selection ratio reaches 300:1, and a smooth and steep straightness of the side wall is close to 90 degrees.
Smart Images

Figure CN118908145A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of device preparation, and in particular to a method for preparing a micro-nano structure. Background Art
[0002] High aspect ratio micro-nano structures are typical structural design forms in micro-nano processing technology, and are widely used in MEMS, photonic crystal research, integrated circuits, etc. High aspect ratio structures have a larger vertical dimension space under the same substrate area, which can significantly improve the performance of the device and provide more possibilities for the development of semiconductor devices.
[0003] Etching, as a key technology in micro-nano manufacturing processes, is often used in the processing of high aspect ratio microstructures. Etching is the process of selectively removing unnecessary materials or parts by chemical or physical methods, which can be divided into patterned etching and non-patterned etching. Among them, patterned etching uses a mask layer to define the surface material area to be etched, and the part not covered by the mask is etched away during the etching process. Patterned etching generally uses materials such as photoresist, metal, silicon oxide or silicon nitride as a mask. Among them, photoresist has poor etching resistance and generally has a low etching selectivity. When preparing high aspect ratio structures, the thickness of the photoresist used needs to be thinner, and the photoresist is not enough to meet the etching requirements during a long etching process. Although etching with metal as mask has a high etching selectivity, during the etching process, the metal mask will be sputtered under the bombardment of high-energy particles, forming a micro-mask, causing the etched surface to be roughened; at the same time, due to the large metal particles, the mask edge uniformity is poor, the side wall smoothness is relatively poor, and the metal mask is not easy to clean, which increases the complexity of the process. The main disadvantages of etching with silicon oxide or silicon nitride as a mask are: the selection of the next layer of material is relatively low, making it difficult to apply it to the processing of high aspect ratio microstructures; the mask edge thickness is relatively thin, and it is easy to form a large "shoulder" on the top of the etched end face due to the inability to fully mask during etching; it is difficult to prepare the mask by lift-off process, and the mask edge prepared by etching method is also relatively rough.
[0004] Therefore, how to manufacture high aspect ratio micro-nano structures with smooth and steep sidewalls and a depth of several microns or even tens of microns is a difficulty that needs to be solved urgently. Summary of the invention
[0005] In view of this, the present disclosure provides a method for preparing a micro-nano structure, comprising: growing a sample layer on a substrate, the sample layer being used to prepare the micro-nano structure; spin-coating a resist on the sample layer; removing part of the resist, the removed part of the resist corresponding to the pattern of the micro-nano structure; depositing an Al2O3 thin film on the surface of the resist, peeling off the resist and the Al2O3 thin film on the surface of the resist, forming an Al2O3 mask on the surface of the sample layer, and using the part of the sample layer not covered by the Al2O3 mask for etching the micro-nano structure; etching the sample layer according to the Al2O3 mask, removing the Al2O3 mask, and obtaining the micro-nano structure.
[0006] Optionally, the spin coating of the resist on the sample layer comprises: cleaning the sample layer; spin coating the resist on the sample layer at a preset rotation speed; and pre-baking the sample layer after the spin coating of the resist.
[0007] Optionally, removing part of the resist includes: exposing and developing the resist to transfer the layout pattern of the micro-nano structure to the resist, and the removed part of the resist is used to form the Al2O3 mask.
[0008] Optionally, the transfer method of the micro-nano structure pattern includes electron beam exposure, ion beam exposure, deep ultraviolet lithography, extreme ultraviolet lithography, nanoimprinting, X-ray lithography, laser direct writing lithography or holographic lithography.
[0009] Optionally, the deposition method of the Al2O3 film includes thermal evaporation, electron beam evaporation, pulsed laser source evaporation deposition, magnetron sputtering, direct current sputtering, radio frequency sputtering, ion beam sputtering or atomic layer deposition.
[0010] Optionally, the etching method of the sample layer includes inductively coupled plasma etching, reactive ion etching, ion beam etching, plasma etching, sputtering and ion milling etching or wet etching.
[0011] Optionally, the Al2O3 mask is formed by a lift-off process.
[0012] Optionally, the Al2O3 mask removal method includes a hot phosphoric acid removal method or an aluminum etchant removal method.
[0013] Optionally, the material of the sample layer includes silicon, germanium, silicon germanium, gallium arsenide, indium antimonide, indium phosphide, gallium phosphide, gallium arsenide, gallium nitride, silicon carbide, cadmium telluride or mercury telluride.
[0014] Optionally, the resist includes electron beam resist, ion beam resist, deep ultraviolet resist, extreme ultraviolet resist or X-ray resist.
[0015] At least one of the above technical solutions adopted in the embodiments of the present disclosure can achieve the following beneficial effects:
[0016] 1. The present invention uses Al2O3 as a mask to prepare micro-nano structures. Al2O3 materials have a high etching resistance to F-based and Cl-based gases, and the etching selectivity ratio can reach 300:1;
[0017] 2. The present invention can realize high-precision transfer of graphics below 100 nanometers. Using Al2O3 as the material in combination with electron beam exposure and lift-off process, it can prepare high-precision and smooth-edge masks with good etching morphology and smooth and steep side walls, thereby being able to manufacture high aspect ratio and high-precision micro-nano structures. The aspect ratio can reach the limit of ICP equipment and the process is simple. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The above and other objects, features and advantages of the present disclosure will become more apparent through the following description of the embodiments of the present disclosure with reference to the accompanying drawings, in which:
[0019] Figure 1 The flowchart of the micro-nano structure preparation method provided by the present disclosure is schematically shown;
[0020] Figure 2 The structure diagram corresponding to the micro-nano structure preparation method provided by the embodiment of the present disclosure is schematically shown;
[0021] Figure 3 A schematic diagram shows a scanning electron microscope top view of a micro-nano structure prepared by the micro-nano structure preparation method provided by an embodiment of the present disclosure;
[0022] Figure 4 A scanning electron microscope side view of a micro-nano structure prepared by the micro-nano structure preparation method provided by an embodiment of the present disclosure is schematically shown.
[0023] Reference numerals:
[0024] 1-substrate; 2-sample layer; 3-resist; 4-Al2O3 film; 5-Al2O3 mask; 6-micro-nano structure. DETAILED DESCRIPTION
[0025] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present disclosure. In the following detailed description, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of the embodiments of the present disclosure. However, it is apparent that one or more embodiments may also be implemented without these specific details. In addition, in the following description, descriptions of known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present disclosure.
[0026] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.
[0027] All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art unless otherwise defined. It should be noted that the terms used herein should be interpreted as having a meaning consistent with the context of this specification and should not be interpreted in an idealized or overly rigid manner.
[0028] Figure 1 A flow chart of a method for preparing a micro-nano structure provided by the present disclosure is schematically shown.
[0029] See also Figure 1 As shown, the present disclosure provides a method for preparing a micro-nano structure, comprising: steps S1 to S5.
[0030] Step S1 , growing a sample layer 2 on a substrate 1 , wherein the sample layer 2 is used to prepare a micro-nano structure 6 .
[0031] As an optional embodiment, the material of the sample layer 2 includes silicon, germanium, silicon germanium, gallium arsenide, indium antimonide, indium phosphide, gallium phosphide, gallium arsenide, gallium nitride, silicon carbide, cadmium telluride or mercury telluride.
[0032] Step S2 , spin coating the resist 3 on the sample layer 2 .
[0033] Figure 2 The structure diagram corresponding to the micro-nano structure preparation method provided by the embodiment of the present disclosure is schematically shown. Figure 2 , Figure 2 (A) in FIG. 1 is a structural diagram obtained after completing step S2.
[0034] As an optional embodiment, the resist 3 includes electron beam resist, ion beam resist, deep ultraviolet resist, extreme ultraviolet resist or X-ray resist.
[0035] As an optional embodiment, step S2 includes: cleaning the sample layer 2; spin coating the resist 3 on the sample layer 2 at a preset rotation speed; and pre-baking the sample layer 1 after the resist 3 is spin coated.
[0036] In a specific embodiment, after the sample layer 2 is cleaned, the resist 3 is spin-coated at a rotation speed of 1500 rpm, and the entire structure after the resist 3 is spin-coated is placed in an oven for pre-baking at a temperature of 150° C. for 15 minutes.
[0037] Step S3, removing part of the resist 3, wherein the removed part of the resist 3 corresponds to the pattern of the micro-nano structure.
[0038] See also Figure 2 As shown, Figure 2 (B) in the figure is the structural diagram obtained after completing step S3.
[0039] As an optional embodiment, removing part of the resist 3 includes: exposing and developing the resist 3 to transfer the pattern of the micro-nano structure on the layout to the resist 3, and the removed part of the resist 3 is used to form an Al2O3 mask 5.
[0040] As an optional embodiment, the transfer method of the micro-nano structure pattern includes electron beam exposure, ion beam exposure, deep ultraviolet lithography, extreme ultraviolet lithography, nanoimprinting, X-ray lithography, laser direct writing lithography or holographic lithography.
[0041] In a specific embodiment, the resist 3 is exposed and developed by electron beam, and the micro-nano structure pattern on the layout is transferred to the resist 3. The electron beam exposure method uses focused electrons with extremely short wavelengths to directly act on the surface of the electron-sensitive resist 3 to draw and form a micro-nano structure that matches the design pattern.
[0042] The electron beam lithography system used in the embodiments of the present disclosure has the advantages of ultra-high resolution (graphic transfer with a limit size of <10 nm) and flexible mapping (direct writing without a mask), and is suitable for the preparation of micro-nano structures.
[0043] Step S4, depositing Al2O3 film 4 on the surface of resist 3, peeling off resist 3 and Al2O3 film 4 on the surface of resist 3, forming Al2O3 mask 5 on the surface of sample layer 3, and the part of sample layer 3 not covered by Al2O3 mask 5 is used for etching of micro-nano structure.
[0044] See also Figure 2 As shown, Figure 2 (C) is a structural diagram obtained after depositing Al2O3 film 4 on the surface of resist 3; Figure 2 (D) in the figure is a structural diagram after an Al2O3 mask 5 is formed on the surface of the sample layer 3.
[0045] As an optional embodiment, the deposition method of the Al2O3 film 4 includes thermal evaporation, electron beam evaporation, pulsed laser source evaporation deposition, magnetron sputtering, DC sputtering, radio frequency sputtering, ion beam sputtering or atomic layer deposition.
[0046] In a specific embodiment, the Al2O3 film 4 is deposited by ion beam sputtering, and the background vacuum is 2×10 -5 Pa, the vacuum degree during deposition is (2.5-3.2)×10-2 Pa, ion beam energy of 600eV, and deposition rate of 0.04nm / s, Al2O3 film 4 was deposited on the surface of resist 3. The main component of the target material is Al2O3 (98%); the current density of the target is 0.5mA / cm 2 ; The energy of the second ion source is 100-600eV.
[0047] As an optional embodiment, the Al2O3 mask 5 is formed by a lift-off process.
[0048] In a specific embodiment, a lift-off process is used to remove the resist 3 , and the Al 2 O 3 film 4 on the surface of the resist 3 is peeled off, so that an Al 2 O 3 mask 5 is formed on the surface of the sample layer 2 .
[0049] In the embodiment of the present disclosure, a lift-off process is used to form the Al2O3 mask 5. Compared with other graphic transfer methods, the lift-off process is simpler and easier to implement, and can prepare a high-precision mask with smooth edges, which is convenient for further manufacturing of high-aspect-ratio, high-precision micro-nano structures.
[0050] Figure 3 A scanning electron microscope top view of a micro-nano structure prepared by the micro-nano structure preparation method provided by an embodiment of the present disclosure is schematically shown.
[0051] Figure 4 A scanning electron microscope side view of a micro-nano structure prepared by the micro-nano structure preparation method provided by an embodiment of the present disclosure is schematically shown.
[0052] Step S5, etching the sample layer 2 according to the Al2O3 mask 5, removing the Al2O3 mask 5, and obtaining the micro-nano structure 6. The micro-nano structure obtained by the micro-nano structure preparation method provided in the embodiment of the present disclosure is as shown in Figure 3 and Figure 4 shown.
[0053] See also Figure 2 As shown, Figure 2 (E) is a structural diagram after etching the sample layer 2 according to the Al2O3 mask 5; Figure 2 (F) in the figure is a structural diagram of the prepared micro-nanostructure.
[0054] As an optional embodiment, the etching method for etching the sample layer 2 includes inductively coupled plasma etching, reactive ion etching, ion beam etching, plasma etching, sputtering and ion milling etching or wet etching.
[0055] In a specific embodiment, taking GaN samples as an example, ICP (Inductively Coupled Plasma) dry etching is adopted, the chamber environment temperature is set to 12°C at the top temperature, 120°C at the coil side wall temperature, 70°C at the lower electrode side wall temperature, 20°C at the electrode temperature, and the helium cooling pressure at the back of the electrostatic chuck electrode is 7000mTorr, at which time the helium flow rate is stable between 4.5sccm and 5.5sccm. Cl2 / Ar gas is selected, the flow rates of Cl2 and Ar are 48sccm and 12sccm respectively, the gas pressure in the chamber is 7mTorr, the electrode bias RF1 power is 200W, and the ICP RF power is 600W. Under this etching condition, an etching rate of 441.3nm / min can be achieved, and the sidewalls of the etched structure are smooth, with a steepness close to 90 degrees.
[0056] As an optional embodiment, the method for removing the Al2O3 mask 5 includes a hot phosphoric acid removal method or an aluminum etchant removal method.
[0057] As an optional embodiment, the material of the sample layer 2 includes silicon, germanium, silicon germanium, gallium arsenide, indium antimonide, indium phosphide, gallium phosphide, gallium arsenide, gallium nitride, silicon carbide, cadmium telluride or mercury telluride.
[0058] In summary, the present invention uses Al2O3 as a mask to prepare micro-nano structures, and cooperates with electron beam exposure and lift-off process to prepare high-precision and smooth-edge masks, good etching morphology, smooth and steep side walls, thereby being able to manufacture high aspect ratio and high-precision micro-nano structures. The aspect ratio can reach the limit of ICP equipment, and the process is simple.
[0059] It will be appreciated by those skilled in the art that the features described in the various embodiments and / or claims of the present disclosure may be combined and / or combined in a variety of ways, even if such combinations and / or combinations are not explicitly described in the present disclosure. In particular, the features described in the various embodiments and / or claims of the present disclosure may be combined and / or combined in a variety of ways without departing from the spirit and teachings of the present disclosure. All of these combinations and / or combinations fall within the scope of the present disclosure.
[0060] Although the present disclosure has been shown and described with reference to specific exemplary embodiments of the present disclosure, it should be understood by those skilled in the art that various changes in form and details may be made to the present disclosure without departing from the spirit and scope of the present disclosure as defined by the appended claims and their equivalents. Therefore, the scope of the present disclosure should not be limited to the above-mentioned embodiments, but should be determined not only by the appended claims, but also by the equivalents of the appended claims.
Claims
1. A method for preparing a micro-nano structure, It is characterized in that include: Growing a sample layer (2) on a substrate (1), wherein the sample layer (2) is used to prepare the micro-nano structure; Spin coating a resist (3) on the sample layer (2); Removing part of the resist (3), wherein the removed part of the resist (3) corresponds to the pattern of the micro-nano structure; Al is deposited on the surface of the resist (3) 2 O 3 The film (4) is used to bond the resist (3) to the Al 2 O 3 The film (4) is peeled off, and the surface of the sample layer (3) forms Al 2 O 3 mask (5), the sample layer (2) is not covered with Al 2 O 3 The portion covered by the mask (5) is used for etching the micro-nano structure; According to the Al 2 O 3 The mask (5) etches the sample layer (2) to remove the Al 2 O 3 A mask (5) is formed to obtain the micro-nano structure (6).
2. The method for preparing a micro-nano structure according to claim 1, It is characterized in that The step of spin coating the resist (3) on the sample layer (2) comprises: Cleaning the sample layer (2); Spin coating a resist (3) on the sample layer (2) at a preset rotation speed; The sample layer (1) after spin coating the resist (3) is pre-baked.
3. The method for preparing a micro-nano structure according to claim 1, It is characterized in that The removing part of the resist (3) comprises: The resist (3) is exposed and developed to transfer the pattern of the micro-nano structure on the layout to the resist (3), and the removed portion of the resist (3) is used to form the Al 2 O 3 Mask (5).
4. The method for preparing a micro-nano structure according to claim 3, It is characterized in that The transfer method of the layout pattern of the micro-nano structure includes electron beam exposure, ion beam exposure, deep ultraviolet lithography, extreme ultraviolet lithography, nanoimprinting, X-ray lithography, laser direct writing lithography or holographic lithography.
5. The method for preparing a micro-nano structure according to claim 1, It is characterized in that The Al 2 O 3 The deposition method of the thin film (4) includes thermal evaporation, electron beam evaporation, pulsed laser source evaporation deposition, magnetron sputtering, direct current sputtering, radio frequency sputtering, ion beam sputtering or atomic layer deposition.
6. The method for preparing a micro-nano structure according to claim 1, It is characterized in that The etching method for etching the sample layer (2) includes inductively coupled plasma etching, reactive ion etching, ion beam etching, plasma etching, sputtering and ion milling etching or wet etching.
7. The method for preparing a micro-nano structure according to claim 1, It is characterized in that The Al 2 O 3 The mask (5) is formed by a lift-off process.
8. The method for preparing a micro-nano structure according to claim 1, It is characterized in that The Al 2 O 3 The mask (5) is removed by a method including a hot phosphoric acid removal method or an aluminum etchant removal method.
9. The method for preparing a micro-nano structure according to claim 1, It is characterized in that The material of the sample layer (2) includes silicon, germanium, silicon germanium, gallium arsenide, indium antimonide, indium phosphide, gallium phosphide, gallium arsenide, gallium nitride, silicon carbide, cadmium telluride or mercury telluride.
10. The method for preparing a micro-nano structure according to claim 1, It is characterized in that The resist (3) includes electron beam resist, ion beam resist, deep ultraviolet resist, extreme ultraviolet resist or X-ray resist.