Method for preparing high-purity iron phosphate by extracting phosphorus from phosphogypsum
Through the leaching, adsorption and elution and hydrothermal reaction steps, the purity and utilization rate of iron phosphate were successfully improved, the environmental pollution and resource waste caused by the storage of phosphogypsum were solved, and high-value utilization was achieved.
Patent Information
- Application Number
- CN202411005670.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The storage of phosphogypsum leads to environmental pollution and waste of resources. It is difficult for the existing technology to effectively utilize the iron phosphate resources in it, resulting in a low comprehensive utilization rate.
Through the leaching, adsorption and elution and hydrothermal reaction steps, high-purity iron phosphate is prepared using the phosphorus elements in the phosphogypsum, including mixing the phosphogypsum with the leaching agent and shaking, filtering, and adsorption and elution using the ZrO2 membrane to regulate After pH value, hydrothermal reaction was carried out, and finally high-purity iron phosphate was obtained by calcination.
It improves the leaching rate of active phosphorus of phosphogypsum, improves the purity of high-purity phosphorus products, realizes the high-value utilization of iron phosphate, reduces environmental pollution, and meets the industry standard iron, phosphorus content and iron-phosphorus molar ratio .
Smart Images

Figure CN118908164A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of phosphogypsum resource utilization, and in particular to a method for extracting phosphorus from phosphogypsum to prepare high-purity iron phosphate. Background Art
[0002] Phosphogypsum is an industrial waste residue generated during the production of wet phosphoric acid. According to statistics, the global stockpile of phosphogypsum has reached 7 billion tons. Large-scale storage of phosphogypsum not only wastes land, but also seriously pollutes the environment. Phosphogypsum leachate dissolves underground rock formations and interacts strongly with surface water and groundwater, exacerbating the flow of impurity elements in phosphogypsum into groundwater, thus causing serious water pollution incidents. Data show that algal blooms occur when the phosphorus concentration in the water is 0.035 mg / L. Therefore, the recovery of phosphorus resources from phosphogypsum can control the total phosphorus pollution problem in the water environment from the source.
[0003] Phosphogypsum is a fine powdery solid. It is acidic and slightly soluble in water. It can be dissolved in solvents such as ammonium salts, acids and glycerol. Its color is generally light gray, yellowish white or dark gray. Phosphogypsum has a complex composition and contains elements such as silicon, iron, titanium, magnesium, aluminum, phosphorus, fluorine and manganese. Impurities such as fluoride, phosphate and heavy metals contained in it are the main elements of environmental pollution during the storage process. At present, a large amount of phosphogypsum is stored in large open-air sites around the world without any pretreatment. It not only occupies a large amount of land area, but also releases pollutants into the atmosphere and water environment, seriously affecting the environment. Therefore, the environmental and management issues brought about by the storage of phosphogypsum have attracted great attention from the world.
[0004] Due to the immaturity of phosphogypsum pretreatment technology, its comprehensive utilization has become a global problem. At present, the global comprehensive utilization rate of phosphogypsum has been low for a long time, only about 25%. The focus of comprehensive utilization of phosphogypsum is related to the economic development of each country. In a few countries, due to the lack of phosphorus resources, the comprehensive utilization rate of phosphogypsum is close to 100%, mainly used to make cement retarders for building materials. In most countries, due to the rich phosphate resources and the high content of harmful and toxic substances in phosphogypsum, the comprehensive utilization of phosphogypsum has not been developed, resulting in a low comprehensive utilization rate, and most of them are stored or discharged into the sea for treatment.
[0005] With the rapid development of new energy vehicles and electric energy storage systems, lithium iron phosphate batteries have attracted much attention due to their high safety, long life and low environmental impact. As the precursor of lithium iron phosphate, the physical and chemical properties of iron phosphate, such as its main components, iron-phosphorus molar ratio, micromorphology, and crystal structure, are key factors in determining the electrochemical performance of lithium iron phosphate batteries. Therefore, how to process phosphogypsum as a resource to obtain high-value-added iron phosphate products is an urgent problem that technicians in this field need to solve. Summary of the invention
[0006] The purpose of the present invention is to provide a method for extracting phosphorus from phosphogypsum to prepare high-purity iron phosphate, so as to solve the problems existing in the above-mentioned prior art.
[0007] To achieve the above object, the present invention provides the following solutions:
[0008] One of the technical solutions of the present invention is to provide a method for extracting phosphorus from phosphogypsum to prepare high-purity iron phosphate, the steps comprising:
[0009] Extracting the phosphogypsum to obtain an extract;
[0010] Adsorbing and eluting the extract to obtain a purified solution;
[0011] The purified solution is used as a phosphorus source, ferric sulfate is used as an iron source, the pH value is adjusted, and a precipitation product is obtained after a hydrothermal reaction;
[0012] The precipitated product is washed and calcined to obtain the high-purity iron phosphate.
[0013] Further, the leaching step comprises:
[0014] The phosphogypsum and the leaching agent are mixed, shaken, and filtered to obtain the leaching solution.
[0015] Preferably, the leaching agent is water, sulfuric acid solution, hydrochloric acid solution or nitric acid solution, more preferably sulfuric acid solution.
[0016] More preferably, the concentration of the sulfuric acid solution, the hydrochloric acid solution and the nitric acid solution is 0-0.2M and is not 0, and is particularly preferably 0.1M.
[0017] Preferably, the liquid-to-solid ratio of the leaching agent to phosphogypsum is 10-40 mL / g, more preferably 40 mL / g.
[0018] Preferably, the extraction time is not less than 10 min, more preferably 10 min.
[0019] Further, the adsorption and elution step comprises:
[0020] The leaching solution is adsorbed by a ZrO2 membrane and then eluted by a sodium hydroxide solution to obtain the purified solution.
[0021] Preferably, during the adsorption, the pH of the extract is adjusted to 1-3, more preferably 2.
[0022] Preferably, the adsorption time is not less than 4 hours, more preferably 8 hours.
[0023] Preferably, the pH value of the sodium hydroxide solution is 14.
[0024] Preferably, the elution time is not less than 60 min, more preferably 60 min.
[0025] Furthermore, the molar ratio of iron to phosphorus in the iron source and the phosphorus source is 1:1.
[0026] Furthermore, the pH value is adjusted to adjust the pH value of the mixed system of the phosphorus source and the iron source to 1-2, preferably 1.6.
[0027] Furthermore, the hydrothermal reaction temperature is not less than 80°C, preferably 80°C.
[0028] Furthermore, the hydrothermal reaction time is not less than 60 min, preferably 60 min.
[0029] Furthermore, the washing is washing with water at least once.
[0030] Furthermore, the calcination temperature is 750°C, the heating rate is 10°C / min, and the calcination time is 3h.
[0031] The second technical solution of the present invention is to provide a method for recycling phosphogypsum, the steps comprising:
[0032] Extracting the phosphogypsum to obtain an extract;
[0033] Adsorbing and eluting the extract to obtain a purified solution;
[0034] The purified solution is used as a phosphorus source, ferric sulfate is used as an iron source, the pH value is adjusted, and a precipitation product is obtained after a hydrothermal reaction;
[0035] The precipitated product is washed and calcined to obtain the high-purity iron phosphate.
[0036] The present invention discloses the following technical effects:
[0037] The present invention can improve the leaching rate of active phosphorus in phosphogypsum by limiting the steps of leaching and adsorption elution, and then obtain a high-concentration phosphate solution through adsorption elution, thereby improving the purity of a high-purity phosphorus product recovered from the leaching solution.
[0038] The iron phosphate prepared by the preparation method of the present invention has iron and phosphorus contents and an iron-phosphorus molar ratio that meet industry standards. The phosphorus element in phosphogypsum is efficiently utilized through a hydrothermal method, thereby achieving high-value utilization and reducing the pollution of phosphogypsum to the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 The effects of different leaching agents on the leaching rates of phosphorus and metal elements in Example 1, wherein a is the effect of the type of leaching agent on the phosphorus leaching rate, and b is the effect of the type of solvent on the leaching rate of metal elements;
[0041] Figure 2 The effect of different sulfuric acid concentrations on the phosphorus leaching rate of phosphogypsum, where a is the effect of sulfuric acid solution concentration on the phosphorus leaching rate, and b is the pH before and after leaching;
[0042] Figure 3 The effect of different liquid-to-solid ratios on phosphorus leaching rate;
[0043] Figure 4 The effect of different dissolution time on phosphorus leaching rate, where a is the effect of dissolution time on phosphorus leaching rate, and b is the comparison of pH values before and after leaching;
[0044] Figure 5 The effect of different pH values on phosphorus adsorption efficiency of ZrO2 membrane;
[0045] Figure 6 The effect of different adsorption time on phosphorus adsorption efficiency of ZrO2 membrane;
[0046] Figure 7 The effect of different eluent pH values on the desorption of ZrO2 membrane after adsorption;
[0047] Figure 8 The effect of different elution time on the desorption effect of ZrO2 film after adsorption;
[0048] Fig. 9 The SEM images and EDS images of the ZrO2 film before adsorption, after adsorption and after elution in Example 9, wherein a is the SEM image before adsorption, b is the EDS image before adsorption, c is the SEM image after adsorption, d is the EDS image after adsorption, e is the SEM image after elution, and f is the EDS image after elution;
[0049] Fig.10 The XPS graphs of the ZrO2 film before adsorption (original film), after adsorption and after elution in Example 9, wherein a is in the range of 0 to 1200 eV, and b is in the range of 124 to 142 eV;
[0050] Fig.11The effects of different pH values of the purified solution on the phosphorus recovery rate and the iron-phosphorus content in the ferric phosphate in Example 10, wherein a represents the effect on the phosphorus recovery rate, and b represents the effect on the iron-phosphorus content in the ferric phosphate;
[0051] Fig.12 The morphological distribution of phosphate in the purified solution under different pH conditions in Example 10;
[0052] Fig.13 This is a comparison diagram of the products prepared at different pH values of the purified solution in Example 10 before and after calcination;
[0053] Fig.14 The effects of different hydrothermal reaction temperatures on the phosphorus recovery rate in the purified solution and the iron-phosphorus content in the ferric phosphate in Example 11, wherein a represents the effect on the phosphorus recovery rate, and b represents the effect on the iron-phosphorus content in the ferric phosphate;
[0054] Fig.15 The effects of different hydrothermal reaction times on the phosphorus recovery rate in the purified solution and the iron-phosphorus content in the ferric phosphate in Example 11, wherein a represents the effect on the phosphorus recovery rate, and b represents the effect on the iron-phosphorus content in the ferric phosphate;
[0055] Fig.16 The effects of different iron-phosphorus molar ratios on the phosphorus recovery rate in the purified solution and the iron-phosphorus content in the ferric phosphate in Example 11, wherein a represents the effect on the phosphorus recovery rate, and b represents the effect on the iron-phosphorus content in the ferric phosphate;
[0056] Fig.17 The XRD diagram of the iron phosphate prepared in Example 14, wherein a is the XRD diagram of the uncalcined product and the product calcined at 450°C, and b is the XRD diagram of the product calcined at 750°C;
[0057] Fig.18 The SEM images and EDS images of the iron phosphate obtained under calcination conditions at 750° C. and commercial iron phosphate in Example 14, wherein a is the SEM image of the iron phosphate obtained under calcination conditions at 750° C., b is the EDS image of the iron phosphate obtained under calcination conditions at 750° C., c is the SEM image of commercial iron phosphate, and d is the EDS image of commercial iron phosphate;
[0058] Fig.19 This is the XPS analysis of the iron phosphate obtained in Example 14 under calcination conditions at 750°C and commercial iron phosphate, wherein a is the elemental characteristic peak of the iron phosphate obtained in Example 14 under calcination conditions at 750°C and commercial iron phosphate, b is the Fe2p XPS spectrum, c is the P2p XPS spectrum, and d is the O1s XPS spectrum. DETAILED DESCRIPTION
[0059] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0060] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0061] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0062] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0063] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0064] The phosphogypsum used in the present invention is collected from the Jiaoyishan slag field in Guiyang City, Guizhou Province (the main source of total phosphorus pollution in Spring No. 34 in the Wujiang River Basin). The phosphogypsum sample is dried before use, ground to 325 mesh, and set aside. The main element composition is shown in Table 1.
[0065] Table 1
[0066]
[0067] In a specific embodiment of the present invention, the industry standards for the iron content, phosphorus content, and iron-phosphorus molar ratio of the ferric phosphate mentioned are shown in Table 2.
[0068] Table 2
[0069]
[0070] Example 1
[0071] The preparation steps of phosphogypsum extract are as follows:
[0072] The leaching agent (water, 0.1M sulfuric acid solution, 0.1M hydrochloric acid solution or 0.1M nitric acid solution) is mixed with phosphogypsum at a liquid-to-solid ratio of 20mL / g, placed on a horizontal shaker, shaken for 30 minutes, and then filtered through a 0.45μm filter membrane to obtain a supernatant, which is the leaching solution.
[0073] Example 2
[0074] The preparation steps of phosphogypsum extract are as follows:
[0075] Phosphogypsum and a leaching agent (0M, 0.1M, 0.2M, 0.3M, 0.4M or 0.5M sulfuric acid solution) were mixed at a liquid-to-solid ratio of 20mL / g, placed on a horizontal shaker, shaken for 30 minutes, and then filtered through a 0.45μm filter membrane to obtain a supernatant, which is the leaching solution.
[0076] Example 3
[0077] The preparation steps of phosphogypsum extract are as follows:
[0078] The leaching agent (0.1M sulfuric acid solution) and phosphogypsum are mixed at a liquid-to-solid ratio of 10mL / g, 20mL / g, 30mL / g, 40mL / g, 50mL / g, 60mL / g, 70mL / g or 80mL / g, placed on a horizontal shaker, shaken for 30 minutes, and then filtered through a 0.45μm filter membrane to obtain a supernatant, which is the leaching solution.
[0079] Example 4
[0080] The preparation steps of phosphogypsum extract are as follows:
[0081] The leaching agent (0.1M sulfuric acid solution) and phosphogypsum were mixed at a liquid-to-solid ratio of 40mL / g, placed on a horizontal shaker, and oscillated for 2min, 10min, 30min, 1h, 2h, 4h, 6h, 8h, 16h or 12h, and then filtered through a 0.45μm filter membrane to obtain the supernatant, which is the leaching solution.
[0082] Example 5
[0083] Adsorption of phosphogypsum extract:
[0084] S1. Mix the leaching agent (0.1M sulfuric acid solution) and phosphogypsum at a liquid-solid ratio of 40 mL / g, place on a horizontal shaker, shake for 10 min, and then filter with a 0.45 μm filter membrane to obtain a supernatant, which is the leaching solution;
[0085] S2. Take 10 mL of the extract and adjust the pH to 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 or 12 with hydrochloric acid and sodium hydroxide. Put the ZrO2 membrane into centrifuge tubes with different pH extracts respectively, place them in a horizontal shaker and shake at T = 25°C and r = 180r / min for 1 hour. After the shaking, take out the ZrO2 membrane to complete the adsorption of the phosphogypsum extract by the ZrO2 membrane.
[0086] Example 6
[0087] Adsorption of phosphogypsum extract:
[0088] S1. Mix the leaching agent (0.1M sulfuric acid solution) and phosphogypsum at a liquid-solid ratio of 40 mL / g, place on a horizontal shaker, shake for 10 min, and then filter with a 0.45 μm filter membrane to obtain a supernatant, which is the leaching solution;
[0089] S2. Take 10 mL of the extract and the ZrO2 membrane and put them into a centrifuge tube. Place it in a horizontal shaker and shake it at T = 25 ° C and r = 180 r / min for 0.5 h, 1 h, 2 h, 4 h, 6 h, 8 h, 12 h, 16 h or 20 h. After the shaking, take out the ZrO2 membrane to complete the adsorption of the phosphogypsum extract by the ZrO2 membrane.
[0090] Example 7
[0091] Adsorption and elution of phosphogypsum extract:
[0092] S1. Mix the leaching agent (0.1M sulfuric acid solution) and phosphogypsum at a liquid-solid ratio of 40 mL / g, place on a horizontal shaker, shake for 10 min, and then filter with a 0.45 μm filter membrane to obtain a supernatant, which is the leaching solution;
[0093] S2, take 10mL of the extract and the ZrO2 membrane into a centrifuge tube, place it in a horizontal shaker and shake it for 8 hours at T = 25°C and r = 180r / min. After the shaking is completed, take out the ZrO2 membrane to complete the adsorption of the phosphogypsum extract by the ZrO2 membrane;
[0094] S3. Elute the adsorbed ZrO2 membrane with eluents of different pH values (use hydrochloric acid or sodium hydroxide to prepare solutions with pH values of 2, 4, 6, 8, 10, 12, and 14). Put 15 mL of the eluent and the adsorbed ZrO2 membrane into a centrifuge tube, and place the centrifuge tube on a horizontal shaker and shake it gently for 60 minutes. After the shaking, take out the ZrO2 membrane, filter the desorption liquid through a filter membrane with a pore size of 0.45 μm, complete the desorption process, and obtain a purified liquid.
[0095] Example 8
[0096] Adsorption and elution of phosphogypsum extract:
[0097] S1. Mix the leaching agent (0.1M sulfuric acid solution) and phosphogypsum at a liquid-solid ratio of 40 mL / g, place on a horizontal shaker, shake for 10 min, and then filter with a 0.45 μm filter membrane to obtain a supernatant, which is the leaching solution;
[0098] S2, take 10mL of the extract and the ZrO2 membrane into a centrifuge tube, place it in a horizontal shaker and shake it for 8 hours at T = 25°C and r = 180r / min. After the shaking is completed, take out the ZrO2 membrane to complete the adsorption of the phosphogypsum extract by the ZrO2 membrane;
[0099] S3. The adsorbed ZrO2 membrane is eluted with an eluent of pH 14 prepared with sodium hydroxide. 15 mL of the eluent and the adsorbed ZrO2 membrane are put into a centrifuge tube, and the centrifuge tube is placed on a horizontal shaker and gently shaken for 20 min, 40 min, 60 min, 80 min, 100 min, 120 min or 140 min. After the shaking, the ZrO2 membrane is taken out and the desorption liquid is filtered through a filter membrane with a pore size of 0.45 μm to complete the desorption process and obtain a purified liquid.
[0100] Example 9
[0101] Adsorption and elution of phosphogypsum extract:
[0102] S1. Mix the leaching agent (0.1M sulfuric acid solution) and phosphogypsum at a liquid-solid ratio of 40 mL / g, place on a horizontal shaker, shake for 10 min, and then filter with a 0.45 μm filter membrane to obtain a supernatant, which is the leaching solution;
[0103] S2, take 10mL of the extract and the ZrO2 membrane into a centrifuge tube, place it in a horizontal shaker and shake it for 8 hours at T = 25°C and r = 180r / min. After the shaking is completed, take out the ZrO2 membrane to complete the adsorption of the phosphogypsum extract by the ZrO2 membrane;
[0104] S3. The adsorbed ZrO2 membrane is eluted with an eluent of pH 14 prepared with sodium hydroxide. 15 mL of the eluent and the adsorbed ZrO2 membrane are placed in a centrifuge tube, and the centrifuge tube is placed on a horizontal shaker and gently shaken for 60 minutes. After the shaking, the ZrO2 membrane is taken out and the desorption liquid is filtered through a filter membrane with a pore size of 0.45 μm to complete the desorption process and obtain a purified liquid.
[0105] Example 10
[0106] Preparation of iron phosphate:
[0107] S1. Mix the leaching agent (0.1M sulfuric acid solution) and phosphogypsum at a liquid-solid ratio of 40 mL / g, place on a horizontal shaker, shake for 10 min, and then filter with a 0.45 μm filter membrane to obtain a supernatant, which is the leaching solution;
[0108] S2, take 10mL of the extract and the ZrO2 membrane into a centrifuge tube, place it in a horizontal shaker and shake it for 8 hours at T = 25°C and r = 180r / min. After the shaking is completed, take out the ZrO2 membrane to complete the adsorption of the phosphogypsum extract by the ZrO2 membrane;
[0109] S3, the adsorbed ZrO2 membrane is eluted with an eluent having a pH of 14 prepared with sodium hydroxide, 15 mL of the eluent and the adsorbed ZrO2 membrane are put into a centrifuge tube, and the centrifuge tube is placed on a horizontal shaker for slight shaking for 60 minutes. After the shaking, the ZrO2 membrane is taken out, and the desorption liquid is filtered through a filter membrane with a pore size of 0.45 μm to complete the desorption process and obtain a purified liquid;
[0110] S4. Add Fe2(SO4)3 solution (iron-phosphorus molar ratio of 1:1) to the purified liquid, stir to fully dissolve the mixture, adjust the pH value to 1.6, 2.2, 2.8 or 3.4 with H2SO4 or NaOH solution, then heat at 80°C in a warm water bath for 60 minutes, then centrifuge at 3200 rpm for 10 minutes to collect the solid product and supernatant, wash the solid product three times with deionized water to remove impurities, and finally calcine at 750°C for 3 hours at a heating rate of 10°C / min to obtain crystalline anhydrous iron phosphate.
[0111] Embodiment 11
[0112] Preparation of iron phosphate:
[0113] S1. Mix the leaching agent (0.1M sulfuric acid solution) and phosphogypsum at a liquid-solid ratio of 40 mL / g, place on a horizontal shaker, shake for 10 min, and then filter with a 0.45 μm filter membrane to obtain a supernatant, which is the leaching solution;
[0114] S2, take 10mL of the extract and the ZrO2 membrane into a centrifuge tube, place it in a horizontal shaker and shake it for 8 hours at T = 25°C and r = 180r / min. After the shaking is completed, take out the ZrO2 membrane to complete the adsorption of the phosphogypsum extract by the ZrO2 membrane;
[0115] S3, the adsorbed ZrO2 membrane is eluted with an eluent having a pH of 14 prepared with sodium hydroxide, 15 mL of the eluent and the adsorbed ZrO2 membrane are put into a centrifuge tube, and the centrifuge tube is placed on a horizontal shaker for slight shaking for 60 minutes. After the shaking, the ZrO2 membrane is taken out, and the desorption liquid is filtered through a filter membrane with a pore size of 0.45 μm to complete the desorption process and obtain a purified liquid;
[0116] S4. Add Fe2(SO4)3 solution (iron-phosphorus molar ratio of 1:1) to the purified liquid, stir to fully dissolve the mixture, adjust the pH value to 1.6 with H2SO4 or NaOH solution, and then heat in a warm water bath at 40°C, 60°C, 80°C or 100°C for 60 minutes, then centrifuge at 3200 rpm for 10 minutes to collect the solid product and supernatant, wash the solid product three times with deionized water to remove impurities, and finally calcine at 750°C for 3 hours at a heating rate of 10°C / min to obtain crystalline anhydrous iron phosphate.
[0117] Example 12
[0118] Preparation of iron phosphate:
[0119] S1. Mix the leaching agent (0.1M sulfuric acid solution) and phosphogypsum at a liquid-solid ratio of 40 mL / g, place on a horizontal shaker, shake for 10 min, and then filter with a 0.45 μm filter membrane to obtain a supernatant, which is the leaching solution;
[0120] S2, take 10mL of the extract and the ZrO2 membrane into a centrifuge tube, place it in a horizontal shaker and shake it for 8 hours at T = 25°C and r = 180r / min. After the shaking is completed, take out the ZrO2 membrane to complete the adsorption of the phosphogypsum extract by the ZrO2 membrane;
[0121] S3, the adsorbed ZrO2 membrane is eluted with an eluent having a pH of 14 prepared with sodium hydroxide, 15 mL of the eluent and the adsorbed ZrO2 membrane are put into a centrifuge tube, and the centrifuge tube is placed on a horizontal shaker for slight shaking for 60 minutes. After the shaking, the ZrO2 membrane is taken out, and the desorption liquid is filtered through a filter membrane with a pore size of 0.45 μm to complete the desorption process and obtain a purified liquid;
[0122] S4. Add Fe2(SO4)3 solution (iron-phosphorus molar ratio of 1:1) to the purified solution, stir to fully dissolve the mixture, adjust the pH value to 1.6 with H2SO4 or NaOH solution, and then heat at 80°C in a warm water bath for 30 minutes, 60 minutes, 90 minutes or 120 minutes, then centrifuge at 3200 rpm for 10 minutes to collect the solid product and supernatant, wash the solid product three times with deionized water to remove impurities, and finally calcine at 750°C for 3 hours at a heating rate of 10°C / min to obtain crystalline anhydrous iron phosphate.
[0123] Embodiment 13
[0124] Preparation of iron phosphate:
[0125] S1. Mix the leaching agent (0.1M sulfuric acid solution) and phosphogypsum at a liquid-solid ratio of 40 mL / g, place on a horizontal shaker, shake for 10 min, and then filter with a 0.45 μm filter membrane to obtain a supernatant, which is the leaching solution;
[0126] S2, take 10mL of the extract and the ZrO2 membrane into a centrifuge tube, place it in a horizontal shaker and shake it for 8 hours at T = 25°C and r = 180r / min. After the shaking is completed, take out the ZrO2 membrane to complete the adsorption of the phosphogypsum extract by the ZrO2 membrane;
[0127] S3, the adsorbed ZrO2 membrane is eluted with an eluent having a pH of 14 prepared with sodium hydroxide, 15 mL of the eluent and the adsorbed ZrO2 membrane are put into a centrifuge tube, and the centrifuge tube is placed on a horizontal shaker for slight shaking for 60 minutes. After the shaking, the ZrO2 membrane is taken out, and the desorption liquid is filtered through a filter membrane with a pore size of 0.45 μm to complete the desorption process and obtain a purified liquid;
[0128] S4. Add Fe2(SO4)3 solution (with an iron-phosphorus molar ratio of 1:1, 1.25:1, 1.5:1 or 2:1) to the purified solution, stir to fully dissolve the mixture, adjust the pH value to 1.6 with H2SO4 or NaOH solution, and then heat at 80°C in a warm water bath for 60 minutes, then centrifuge at 3200 rpm for 10 minutes to collect the solid product and supernatant, wash the solid product three times with deionized water to remove impurities, and finally calcine at 750°C for 3 hours at a heating rate of 10°C / min to obtain crystalline anhydrous iron phosphate.
[0129] Embodiment 14
[0130] Preparation of iron phosphate:
[0131] S1. Mix the leaching agent (0.1M sulfuric acid solution) and phosphogypsum at a liquid-solid ratio of 40 mL / g, place on a horizontal shaker, shake for 10 min, and then filter with a 0.45 μm filter membrane to obtain a supernatant, which is the leaching solution;
[0132] S2, take 10mL of the extract and the ZrO2 membrane into a centrifuge tube, place it in a horizontal shaker and shake it for 8 hours at T = 25°C and r = 180r / min. After the shaking is completed, take out the ZrO2 membrane to complete the adsorption of the phosphogypsum extract by the ZrO2 membrane;
[0133] S3, the adsorbed ZrO2 membrane is eluted with an eluent having a pH of 14 prepared with sodium hydroxide, 15 mL of the eluent and the adsorbed ZrO2 membrane are put into a centrifuge tube, and the centrifuge tube is placed on a horizontal shaker for slight shaking for 60 minutes. After the shaking, the ZrO2 membrane is taken out, and the desorption liquid is filtered through a filter membrane with a pore size of 0.45 μm to complete the desorption process and obtain a purified liquid;
[0134] S4. Add Fe2(SO4)3 solution (iron-phosphorus molar ratio of 1:1) to the purified liquid, stir to fully dissolve the mixture, adjust the pH value to 1.6 with H2SO4 or NaOH solution, and then heat at 80°C in a warm water bath for 60 minutes, then centrifuge at 3200 rpm for 10 minutes to collect the solid product and supernatant, wash the solid product three times with deionized water to remove impurities, and finally calcine at 450°C or 750°C at a heating rate of 10°C / min for 3 hours to obtain crystalline anhydrous iron phosphate.
[0135] Test example
[0136] The concentrations of phosphorus and major metal ions (Fe, Mn, Ca, Al) in the leaching solution prepared in Example 1 were analyzed to investigate the effects of different solvents on the leaching rates of phosphorus and metal ions. Figure 1 shown.
[0137] Figure 1 The effects of different leaching agents on the leaching rates of phosphorus and metal elements in Example 1 are shown in Figure 1, where a is the effect of the type of leaching agent on the phosphorus leaching rate, and b is the effect of the type of solvent on the leaching rate of metal elements. Figure 1It can be seen that the leaching efficiency of phosphorus and metal elements by different leaching agents is significantly different. The phosphorus concentration of the leaching solution changes from 1632.6 mg / kg to 3092.7 mg / kg, and the leaching efficiency changes from 32.0% to 60.7%. The main leached metal ions are Al (leaching efficiency: 19.9% to 31.5%), Ca (leaching efficiency: 3.5% to 7.6%), Mg (leaching efficiency: 7.6% to 12.1%) and Mn (leaching efficiency: 0.7% to 1.0%). The leaching efficiency of acid for phosphorus and metal elements is significantly better than that of water because acid can provide H + OH - Hydrochloric acid, sulfuric acid and nitric acid are all strong acids that can completely dissociate into H + , but at the same concentration, sulfuric acid contains more H + Therefore, the phosphorus extraction rate is the highest when sulfuric acid is used as a solvent. The anions in phosphogypsum are mainly SO4 2- and F - In order to avoid the introduction of new impurities and considering the extraction efficiency and cost, sulfuric acid solution was selected as the optimal leaching agent.
[0138] The phosphorus concentration in the leaching solution prepared in Example 2 was analyzed, and the pH value before and after leaching was recorded to determine the effect of the sulfuric acid solution concentration on the phosphorus leaching rate. Figure 2 shown.
[0139] Figure 2 The effect of different sulfuric acid concentrations on the phosphorus leaching rate of phosphogypsum, where a is the effect of sulfuric acid solution concentration on the phosphorus leaching rate, and b is the pH before and after leaching. (The initial pH value of the leaching solution in b refers to the pH value of the leaching agent, and the final pH value of the leaching solution refers to the pH value of the leaching solution) Figure 2 It can be seen that the phosphorus leaching rate in a increases first and then decreases with the increase of sulfuric acid concentration. When the sulfuric acid concentration is 0.1M, most of the water-soluble phosphorus in phosphogypsum is dissolved in the sulfuric acid solution, and the phosphorus leaching rate reaches 62.3%. When the sulfuric acid concentration is greater than 0.2M, continuing to increase the sulfuric acid concentration does not improve the phosphorus leaching efficiency, but instead shows a decreasing trend. This is because when the sulfuric acid concentration is too high, the solution contains a large amount of sulfate ions, which will inhibit the surface OH - With H + Combined with, thus affecting the release of phosphorus-containing anions. The change in solution pH before and after leaching in b, when the concentration is greater than 0.2M, the pH of the leaching solution is less than 1. The results show that when the pH is greater than 1, the phosphorus concentration is negatively correlated with the pH, and when the pH is less than 1, the phosphorus concentration is positively correlated with the pH. Combined with the effect of sulfuric acid concentration on phosphorus leaching rate, sulfuric acid with a concentration of 0.1M was selected as the preferred leaching agent.
[0140] The phosphorus concentration in the leaching solution prepared in Example 3 was analyzed to determine the effect of the liquid-to-solid ratio on phosphorus leaching. The results are as follows: Figure 3 shown.
[0141] Figure 3 The effect of different liquid-solid ratios on phosphorus leaching rate is shown in Figure 3 It can be seen that the liquid-solid ratio is crucial for the efficient extraction of phosphorus leaching rate. As the liquid-solid ratio gradually increases, the phosphorus leaching first gradually increases, and then remains unchanged or decreases. This is mainly because when the liquid-solid ratio increases, the amount of liquid phase increases, which reduces the diffusion resistance and thus increases the solubility of phosphogypsum. When the liquid-solid ratio of the reaction system reaches 40mL / g, the phosphorus leaching rate reaches 83.1±6.3%. The liquid-solid ratio continues to increase, and the phosphorus leaching rate fluctuates little. In order to reduce the process cost as much as possible, a liquid-solid ratio of 40mL / g is used as the optimal liquid-solid ratio.
[0142] The phosphorus concentration in the leaching solution prepared in Example 4 was analyzed to determine the effect of dissolution time (oscillation time) on phosphorus leaching, and the pH value before and after leaching was recorded. The results are as follows: Figure 4 shown.
[0143] Figure 4 The effect of different dissolution time on phosphorus leaching rate, where a is the effect of dissolution time on phosphorus leaching rate, and b is the comparison of pH values before and after leaching. (The initial pH value of the leaching solution in b refers to the pH value of the leaching agent, and the final pH value of the leaching solution refers to the pH value of the leaching solution) Figure 4 It can be seen that the phosphorus leaching rate can reach 81.2±2.3% within 10 minutes. When the reaction time is greater than 10 minutes, the phosphorus leaching rate tends to be stable, and the effect of extending the time on the phosphorus leaching rate is not significant. Therefore, the optimal leaching time is selected as 10 minutes.
[0144] The method of Example 5 was used to adsorb the extract, and the adsorbed solution was filtered through a filter membrane with a pore size of 0.45 μm. The phosphorus content in the filtrate was determined by spectrophotometry to determine the optimal adsorption pH. Three parallel tests were conducted for each pH to investigate the effect of different pH on phosphorus adsorption efficiency. The results are as follows: Figure 5 shown.
[0145] Figure 5 The effect of different pH values on the phosphorus adsorption efficiency of ZrO2 membrane is shown in Figure 5 It can be seen that the pH value can determine the proton concentration in the solution, thereby affecting the phosphorus adsorption capacity of the ZrO2 membrane. The phosphorus adsorption efficiency of the ZrO2 membrane increases first and then decreases with the increase of pH. When the pH is 2, the phosphorus adsorption efficiency reaches 64.4±1.5%. When the pH continues to increase to 12, the phosphorus adsorption efficiency decreases significantly to 45.8±2.0%. The pH range of the phosphogypsum extract is 1~2 ( Figure 4b), indicating that the phosphogypsum extract can be used in the phosphorus adsorption process of ZrO2 membrane without any treatment.
[0146] The method of Example 6 was used to adsorb the extract, and the adsorbed solution was filtered through a filter membrane with a pore size of 0.45 μm. The phosphorus content in the filtrate was determined by spectrophotometry to determine the optimal adsorption time. Three parallel tests were set for each adsorption time to investigate the effect of different adsorption times on phosphorus adsorption efficiency. The results are as follows: Figure 6 shown.
[0147] Figure 6 The effect of different adsorption time on phosphorus adsorption efficiency of ZrO2 membrane is shown in Figure 2. Figure 6 It can be seen that the adsorption efficiency of ZrO2 membrane for phosphorus increases continuously with the extension of oscillation time. The phosphorus adsorption efficiency can reach 85.68±0.72% in 4 hours, and finally reaches adsorption equilibrium in 8 hours, and the adsorption rate reaches 97.0±0.4%.
[0148] The phosphorus content in the filtrate of the purified solution prepared in Example 7 was measured by spectrophotometry to determine the optimal elution pH value. The results are as follows: Figure 7 shown.
[0149] Figure 7 The effect of different eluent pH values on the desorption of ZrO2 membrane after adsorption is shown in Figure 2. Figure 7 It can be seen that in the phosphate elution process, as the pH increases, the elution rate of phosphorus shows a trend of first slowly rising and then sharply rising. In the process of pH increasing from 12 to 14, the elution rate of phosphorus shows an obvious upward trend, from 17.46% to 92.83%. Therefore, it is more appropriate to choose pH = 14 (1M NaOH solution) for the elution experiment.
[0150] The purified solution prepared in Example 8 was used to measure the phosphorus content in the filtrate by spectrophotometry to determine the optimal elution time. The results are as follows: Figure 8 shown.
[0151] Figure 8 The effect of different elution times on the desorption effect of ZrO2 membrane after adsorption is shown in Figure 2. Figure 8 It can be seen that with the increase of elution time, the phosphorus removal rate shows a trend of first increasing and then stabilizing. When the elution time is 60 minutes, the phosphorus elution rate reaches 94.5%, after which the phosphorus elution rate gradually stabilizes. Although too long elution time will increase the amount of phosphate eluted, it will cause the entire experimental process to be prolonged and consume a lot of energy. Therefore, 60 minutes is selected as the optimal ZrO2 membrane elution time.
[0152] Fig. 9The SEM images and EDS images of the ZrO2 film before adsorption, after adsorption and after elution in Example 9, wherein a is the SEM image before adsorption, b is the EDS image before adsorption, c is the SEM image after adsorption, d is the EDS image after adsorption, e is the SEM image after elution, and f is the EDS image after elution. Fig. 9 It can be seen that the anions in the ZrO2 film after adsorption, mainly P, F, and S, are evenly distributed on the surface of the film. This is because different anions exist in different forms due to different dissociation constants. Under acidic conditions, phosphate is in the form of protonated H2PO4 - In the form of H2PO4 - When acting as both a hydrogen bond acceptor and a hydrogen bond donor, the adsorbent can simultaneously adsorb phosphate and other anions (SO4 2- 、NO3 - , Cl - and F - ). After eluting the ZrO2 membrane with 1M NaOH solution, Zr and O were found as the main components, with trace elements Na and Ca, indicating that P was successfully eluted and the membrane had good recycling performance and could be reused.
[0153] Fig.10 The XPS graphs of the ZrO2 film before adsorption (original film), after adsorption and after elution in Example 9, where a is in the range of 0 to 1200 eV and b is in the range of 124 to 142 eV. Fig.10 It can be seen that a new P2p peak at 134 eV appears in the XPS spectrum of the ZrO2 film after adsorption, which is direct evidence of the successful adsorption of phosphorus. The adsorption of phosphate in the phosphogypsum extract by the ZrO2 film is mainly due to the hydroxyl groups (≡Zr-OH) on the surface of zirconium oxide reacting with phosphate (H2PO4 - and HPO4 2- ) through ligand exchange and form an inner complex. ZrO2 membrane will also form an outer complex with other anions (chloride, nitrate, fluoride, etc.), but the inner complex has a stronger binding ability than the outer complex.
[0154] Fig.11 The effects of different pH values of the purified solution on the phosphorus recovery rate and the iron-phosphorus content in the ferric phosphate in Example 10, wherein a represents the effect on the phosphorus recovery rate, and b represents the effect on the iron-phosphorus content in the ferric phosphate; Fig.12 The morphological distribution of phosphate in the purified solution under different pH conditions in Example 10; Fig.13 The figure is a comparison of the products prepared from the purified solution at different pH values in Example 10 before and after calcination. Figures 11 to 13 It can be seen that Fig.11In a, as the pH of the reaction system increases, the phosphorus recovery rate gradually increases, and the phosphorus recovery rate changes from 90.1% to 99.2%. This is because the increase in pH promotes the H2PO4 ﹣ Ionization produces PO4 3﹣ ( Fig.12 ), which is conducive to the positive chemical reaction. The color of the hydrated iron phosphate sample changes from light yellow to reddish brown with the increase of pH. This is because both hydrated iron phosphate and iron hydroxide may precipitate with a positive saturation index between pH = 1 and pH = 4. When pH > 2, the precipitation saturation index of iron hydroxide exceeds FePO4·2H2O, and iron hydroxide precipitation will be generated in the prepared sample. After the iron phosphate prepared under different pH conditions is centrifuged, dried, and calcined at high temperature, the color of the anhydrous iron phosphate sample changes to grayish white and grayish black ( Fig.13 ). Fig.11 In b, as the pH increases, the iron content, phosphorus content, and iron-phosphorus molar ratio in ferric phosphate all tend to decrease. This is because as the pH increases, the amount of precipitate increases, and PO4 3- The aggregation of Fe 3+ Competition PO4 3- The formation of a small amount of insoluble impurities. When the pH value is 1.6 and 2.2, the iron content, phosphorus content, and iron-phosphorus molar ratio of iron phosphate are all within the industry standard range; when the pH value is 2.8 and 3.4, the iron-phosphorus molar ratio in iron phosphate is lower than the industry standard range. The pH value of the solution is an important factor affecting the precipitation of FePO4·2H2O. Iron phosphate is only generated when the pH is less than 4 and dominates between pH = 1 and 2. In order to reduce the impurities in the recovered iron phosphate precipitate, the pH value of the system should be adjusted between 1 and 2. Although iron hydroxide can be precipitated at pH = 1 to 2, iron hydroxide is acid-soluble and can be easily redissolved in the solution in a strong acid environment, thereby ensuring the recovery of high-purity iron phosphate precipitates. Although increasing the pH will increase the phosphorus recovery rate of the reaction system, in order to minimize the impurities in the recovered iron phosphate, the pH of the purified solution is controlled at 1.6.
[0155] Fig.14 The effects of different hydrothermal reaction temperatures on the phosphorus recovery rate in the purified solution and the iron-phosphorus content in the ferric phosphate in Example 11 are shown in Table 1, where a represents the effect on the phosphorus recovery rate and b represents the effect on the iron-phosphorus content in the ferric phosphate. Fig.14It can be seen that in a, as the reaction temperature increases, the phosphorus recovery efficiency gradually increases. The phosphorus recovery rates at 40°C, 60°C, 80°C and 100°C are 77.4%, 80.9%, 90.1% and 91.5%, respectively. This is because as the reaction temperature increases, the Gibbs free energy of the reaction to generate iron phosphate precipitation gradually becomes negative. The increase in temperature can overcome the kinetic energy barrier and promote the Brownian motion between ions in the solution, thereby accelerating the rate of the chemical reaction and making the reaction proceed in the positive direction. The results show that the increase in reaction temperature is thermodynamically favorable for the reaction to generate iron phosphate; in b, the iron and phosphorus content in iron phosphate tends to increase with the increase in temperature, and the iron-phosphorus molar ratio tends to increase first and then decrease. When the reaction temperature reaches 80°C, the iron, phosphorus content and iron-phosphorus molar ratio in iron phosphate meet the industry standards. Therefore, 80°C is selected as the reaction temperature for recovering iron phosphate.
[0156] Fig.15 The effects of different hydrothermal reaction times on the phosphorus recovery rate in the purified solution and the iron-phosphorus content in the ferric phosphate in Example 11 are shown in Table 1, where a represents the effect on the phosphorus recovery rate and b represents the effect on the iron-phosphorus content in the ferric phosphate. Fig.15 It can be seen that as the reaction time increases in a, the recovery rate of phosphorus in the purified solution shows a trend of first rising rapidly and then gradually stabilizing, and the phosphorus recovery rate ranges from 76.1 to 90.5%. When the reaction time is greater than 60 minutes, the phosphorus recovery rate is basically stable at more than 90%. It can be found in b that the iron content in iron phosphate has been rising, because the forward reaction is not complete at 30 minutes, and the iron content is low. When the time is 60 minutes and 120 minutes, the iron content and iron-phosphorus ratio in iron phosphate reach the industry standard. In order to save time and electricity costs, the reaction time is controlled at 60 minutes.
[0157] Fig.16 The effects of different iron-phosphorus molar ratios on the phosphorus recovery rate in the purified solution and the iron-phosphorus content in the ferric phosphate in Example 11 are shown in Table 1, where a represents the effect on the phosphorus recovery rate and b represents the effect on the iron-phosphorus content in the ferric phosphate. Fig.16 It can be seen that in a, as the iron-phosphorus ratio of the reaction system increases, the recovery rate of phosphorus in the purified solution shows a gradual upward trend, and the phosphorus recovery rate ranges from 90.1 to 94.3%. The filtered solution under the condition of high iron-phosphorus ratio is light yellow, which indicates that when the reaction pH, temperature and time are optimal, the excess iron source cannot completely react with the phosphate in the purified solution. Combined with b, it can be seen that as the iron-phosphorus molar ratio increases during the reaction, the iron content and iron-phosphorus molar ratio in the iron phosphate sample decrease, and the phosphorus content increases. Only when the iron-phosphorus ratio of the reaction system is 1:1, the iron content, phosphorus content and iron-phosphorus ratio in the iron phosphate meet the industry standards. Therefore, it is more appropriate to select a phosphorus-iron molar feed ratio of 1:1.
[0158] Fig.17The XRD diagram of the iron phosphate prepared in Example 14, wherein a is the XRD diagram of the uncalcined and 450°C calcined products, and b is the XRD diagram of the 750°C calcined product. Fig.17 It can be seen that the XRD spectrum of the iron phosphate in a does not show any characteristic peaks when it is not calcined and calcined at a lower temperature (450°C). This may be because the reaction time is short, resulting in the failure of the prepared iron phosphate to form a good crystal structure. In B, when the calcination temperature is further increased to 750°C, the XRD spectrum shows characteristic peaks corresponding to the FePO4 standard card (PDF#77-0094) at 20.3° and 25.7°, which is a hexagonal crystal structure. The iron phosphate calcined at 750°C shows good crystallinity, indicating that the iron phosphate is transformed from an amorphous structure to a crystalline structure under high-temperature calcination, and it also proves that the iron phosphate product is successfully recovered from phosphogypsum.
[0159] Fig.18 The SEM images and EDS images of the iron phosphate obtained under calcination conditions at 750°C and commercial iron phosphate in Example 14, wherein a is the SEM image of the iron phosphate obtained under calcination conditions at 750°C, b is the EDS image of the iron phosphate obtained under calcination conditions at 750°C, c is the SEM image of commercial iron phosphate, and d is the EDS image of commercial iron phosphate. (Commercial iron phosphate is provided by Shanghai Zhanyun Chemical Co., Ltd., CAS-13463-10-0) Fig.18 It can be seen that from the comparison of a and c, it can be found that from the iron phosphate of Example 14 to the commercial iron phosphate, the particle size of the iron phosphate increases from small to large, indicating that under the process conditions of the present invention, nano-scale spherical iron phosphate can be prepared, and the particle size is smaller, more uniform, and has better dispersion than the commercial iron phosphate; in b and d, the main impurity elements present in the iron phosphate of Example 14 are Na, S, and F. This is because when the ZrO2 membrane is used to adsorb the phosphorus element in the phosphogypsum leachate, the fluorine ions will also be adsorbed and eluted, resulting in a small amount of fluorine in the iron phosphate of Example 14. The fluorine content in the iron phosphate of Example 14 is equivalent to that in the commercial iron phosphate. The small amount of fluorine in the iron phosphate of Example 14 will not affect its commercial quality. The presence of S in the iron phosphate sample of Example 14 is because SO4 will exist in the leachate itself when the phosphogypsum is soaked in sulfuric acid. 2- ions, and part of the S element in the phosphogypsum will be leached, resulting in a large amount of SO4 in the leachate 2- In addition, when 0.1 M NaOH is used as the eluent, during the thermal precipitation of iron phosphate, Na ions will be adsorbed and encapsulated, thus affecting its crystal morphology, size and purity.
[0160] Fig.19The XPS analysis of the iron phosphate obtained by calcining at 750°C and commercial iron phosphate in Example 14, wherein a is the element characteristic peak of the iron phosphate obtained by calcining at 750°C and commercial iron phosphate in Example 14, b is the Fe2p XPS spectrum, c is the P2p XPS spectrum, and d is the O1s XPS spectrum. Fig.19 It can be seen that the elements represented by the characteristic peaks in a are Fe, O, C, and P; b represents the Fe 2p trajectory, and it is found that the iron phosphate obtained in Example 14 under calcination conditions at 750°C has two characteristic peaks at 711.92eV and 725.59eV, and the commercial iron phosphate has two characteristic peaks at 711.84eV and 725.51eV. The dominant valence state of iron in the iron phosphate obtained in Example 14 under calcination conditions at 750°C is +3. In addition, the valence states of Fe 2p, P 2p, and O1s in the iron phosphate obtained in Example 14 under calcination conditions at 750°C are the same as those of Fe 2p, P 2p, and O 1s in the commercial iron phosphate. The above results show that the iron phosphate obtained in Example 14 under calcination conditions at 750°C has a high purity and can reach a commercial level.
[0161] The present invention studies by controlling different reaction conditions, and the optimal process for preparing iron phosphate is pH=1.6, T=80°C, T=60 minutes, Fe / P=1. Under the optimal process conditions, the phosphorus recovery rate reaches 90.1%, and the iron, phosphorus content and iron-phosphorus molar ratio in iron phosphate all meet the industry standards. It is found that the pH, temperature, time and iron-phosphorus molar ratio of the reaction system have a certain influence on the phosphorus recovery rate, the purity of iron phosphate and the iron-phosphorus molar ratio in iron phosphate, among which the pH has a small effect on the phosphorus recovery rate and the iron-phosphorus molar ratio in iron phosphate, but has a large effect on the purity of iron phosphate. Too high pH may produce a large amount of iron hydroxide precipitation, thereby affecting the purity and quality of iron phosphate; the temperature and time have a small effect on the purity of iron phosphate and the iron-phosphorus molar ratio in iron phosphate, but significantly affect the reaction phosphorus recovery rate; the iron-phosphorus molar ratio of the reaction system has a large effect on the iron-phosphorus molar ratio in iron phosphate.
[0162] The iron phosphate prepared under the optimal process conditions is an amorphous structure, which may be due to the short reaction time, resulting in the iron phosphate not forming a good crystal structure. After high-temperature calcination at 750°C, the iron phosphate changes from an amorphous structure to a crystalline structure, which is a hexagonal crystal structure. Under the optimal process, nano-scale spherical iron phosphate can be prepared, and the particle size is smaller than that of commercial iron phosphate, more uniform, and better dispersed, which can reach commercial level.
[0163] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for extracting phosphorus from phosphogypsum to prepare high-purity iron phosphate, characterized in that the steps include: Extracting the phosphogypsum to obtain an extract; Adsorbing and eluting the extract to obtain a purified solution; The purified solution is used as a phosphorus source, ferric sulfate is used as an iron source, the pH value is adjusted, and a precipitation product is obtained after a hydrothermal reaction; The precipitated product is washed and calcined to obtain the high-purity iron phosphate.
2. The method according to claim 1, characterized in that The step of leaching comprises: The phosphogypsum and the leaching agent are mixed, shaken, and filtered to obtain the leaching solution.
3. The method according to claim 2, characterized in that The leaching agent is water, sulfuric acid solution, hydrochloric acid solution or nitric acid solution; the liquid-to-solid ratio of the leaching agent to phosphogypsum is 10-40 mL / g; and the leaching time is not less than 10 minutes.
4. The method according to claim 1, characterized in that: The adsorption and elution steps include: The leaching solution is adsorbed by a ZrO2 membrane and then eluted by a sodium hydroxide solution to obtain the purified solution.
5. The method according to claim 4, characterized in that During the adsorption, the pH of the extract is adjusted to 1-3; the adsorption time is not less than 4 hours; the pH value of the sodium hydroxide solution is 14; and the elution time is not less than 60 minutes.
6. The method according to claim 1, characterized in that The molar ratio of iron to phosphorus in the iron source and the phosphorus source is 1:1; and the pH value is adjusted to adjust the pH value of the mixed system of the phosphorus source and the iron source to 1-2.
7. The method according to claim 1, characterized in that The hydrothermal reaction temperature is not less than 80° C.; the hydrothermal reaction time is not less than 60 min.
8. The method according to claim 1, characterized in that The washing is washing with water at least once.
9. The method according to claim 1, characterized in that: The calcination temperature is 750°C, the heating rate is 10°C / min, and the calcination time is 3h.
10. A method for recycling phosphogypsum, characterized in that the steps include: Extracting the phosphogypsum to obtain an extract; Adsorbing and eluting the extract to obtain a purified solution; The purified solution is used as a phosphorus source, ferric sulfate is used as an iron source, the pH value is adjusted, and a precipitation product is obtained after a hydrothermal reaction; The precipitated product is washed and calcined to obtain the high-purity iron phosphate.
Citation Information
Patent Citations
Method for recovering phosphorus resource and byproduct magnesium ammonium phosphate in phosphogypsum
CN114275756A
Method for preparing battery-grade iron phosphate by decomposing phosphorite with nitric acid
CN115092901A
Method for recycling iron phosphate from ferrophosphorus waste residues
CN116924363A
Method for recovering phosphorus from ardealite leachate to prepare lithium iron phosphate and application