Preparation process of mesoporous carbon

Silicone sol templates are prepared by reacting fluosilicate and calcium carbonate. Combined with hydrofluoric acid treatment, the high specific surface area and small pore size characteristics of mesoporous carbon are achieved, the problem of waste liquid treatment is solved, it is suitable for electrode materials and other fields, and silicon is improved Recycling rate of the source.

CN118908180AActive Publication Date: 2024-11-08ZHEJIANG UNIV OF TECH +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410974118.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing mesoporous carbon preparation process is difficult to achieve the preparation of mesoporous carbon with a high specific surface area, uniform pore size and less than 6 nm, and there is a problem of waste acid and waste alkali liquid treatment, which cannot meet the needs of electrochemical electrode materials.

Method used

The silica sol template is prepared by reacting fluorosilicate and calcium carbonate, and the carbon source is mixed with the silica sol to remove the template using hydrofluoric acid to form mesoporous carbon, and the generated fluorosilicate solution is recycled to achieve silicon and fluorine Recycled application to prepare mesoporous carbon with high specific surface area, large pore volume and small pore size.

Benefits of technology

It realizes the high specific surface area, large pore volume and small pore size characteristics of mesoporous carbon, and basically does not produce waste liquid. It is suitable for strict electrode materials and other fields, provides a solution for waste liquid treatment, and improves the silicon template. Recycling rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908180A_ABST
    Figure CN118908180A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation process of mesoporous carbon with a recyclable silicon source and mesoporous carbon with small aperture and large specific surface area. The preparation process of the mesoporous carbon comprises the following steps: preparing a silicon template: reacting a fluosilicic acid solution with calcium carbonate, and separating calcium fluoride precipitate and silica sol; the pH value of the silica sol is 2-5; the concentration of silicon dioxide in the silica sol is 1-8wt%; preparing a precursor: dissolving a carbon source and organic acid in silica sol, drying, grinding, and carbonizing in an inert atmosphere to obtain a C / Si precursor; the organic acid comprises at least one of oxalic acid, tannic acid, acetic acid and citric acid; the C / Si precursor is treated with hydrofluoric acid, mesoporous carbon and a fluosilicic acid solution are obtained through solid-liquid separation, and the fluosilicic acid solution is used for preparing the silicon template. The mesoporous carbon has a specific surface area of more than 800m < 2 > / g and a pore diameter of less than 6nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mesoporous carbon preparation, and in particular to a process for preparing mesoporous carbon with recyclable silicon source and mesoporous carbon with small pore size and large specific surface area. Background Art

[0002] Mesoporous carbon is a material with high specific surface area, strong adsorption capacity, good electrical conductivity, stable chemical properties, and adjustable surface chemical properties; it has broad application potential in the fields of catalyst carriers, adsorption, hydrogen storage, electrode materials, environment, and medicine. At present, the preparation process of mesoporous carbon is mostly template method, which is divided into hard template method and soft template method. The advantage of the template method is that the prepared mesoporous carbon has a high specific surface area and uniform pore size and regular arrangement; the disadvantage is that the pore size of the mesoporous carbon is limited by the wall thickness of the template, which is difficult to meet the needs of special industries such as electrochemical electrode materials (pore size requirements are below 6nm); and a large amount of waste acid and waste alkali liquid is generated during the template removal process. Therefore, it is necessary to find a preparation process for mesoporous carbon materials with high specific surface area and uniform pore size, starting from cheap raw materials, and reasonably solving the problem of waste acid and waste alkali.

[0003] The patent specification with application number CN202010572464.5 discloses a process for preparing high-purity fluorite by rapid reaction of fluorosilicic acid and calcium carbonate. The patented technology utilizes the reaction of fluorosilicic acid and calcium carbonate to form calcium fluoride at room temperature through a protective agent, and obtains high-purity fluorite powder by separating silicon dioxide from calcium fluoride. The patented technology does not involve the treatment of silicon dioxide.

[0004] The patent specification with application number CN201711329074.X discloses a method for preparing a mesoporous carbon catalyst, which uses phenol-aldehyde as a carbon precursor and commercially available silica sol as a hard template. The carbon / silicon composite material is obtained through sol-gel, drying, and carbonization, and then treated with alkaline solution to make etching and loading proceed simultaneously, and finally dried to obtain an alkaline mesoporous carbon catalyst. This method simplifies the preparation and loading process of mesoporous carbon, but the method still forms alkaline waste liquid, and the pore size of the obtained mesoporous carbon is similar to the silica particle size in the silica sol, with a larger pore size and a smaller specific surface area.

[0005] The patent specification with application number CN200910152795.7 discloses a method for preparing acrylonitrile polymer-based mesoporous carbon, which uses ammonia water to adjust the pH of silica sol with a particle size of 5 to 20 nm, modifies the silica sol with 2-amidinopropane, adds a carbon source and an emulsifier, and then carbonizes and removes the silicon template with hydrofluoric acid to obtain a mesoporous carbon product. The pore size of the mesoporous carbon obtained by this method can be adjusted within the range of 4 to 45 nm, and the pore size depends on the size of the silica particles in the silica sol. The synthetic pore size of the mesoporous carbon is less than 6 nm, and the size of the silicon template particle size must be strictly required to be less than 8 nm; and the method does not involve the treatment of hydrofluoric acid / fluorosilicic acid waste liquid. Summary of the invention

[0006] The present invention provides a process for preparing mesoporous carbon with recyclable silicon source and the corresponding mesoporous carbon, wherein the obtained mesoporous carbon has the characteristics of high specific surface area, large pore volume and small pore size. In the process of preparation, the recycling rate of silicon template is high, the silicon recovery rate is greater than 80%, and basically no waste acid and waste alkali liquid is generated. Moreover, the mesoporous carbon product has good properties such as high specific surface area, large pore volume and small pore size, so that it can be applied to the fields of electrode materials, shape-selective catalysis, selective adsorption, etc., which have strict requirements on pore size.

[0007] A process for preparing mesoporous carbon with recyclable silicon source, comprising:

[0008] Preparation of silicon template: Fluorosilicic acid solution reacts with calcium carbonate to separate calcium fluoride precipitate and silica sol; the pH of the silica sol is 2 to 5; the concentration of silicon dioxide in the silica sol is 1 to 8 wt%;

[0009] Preparing a precursor: dissolving a carbon source and an organic acid in a silica sol, drying, grinding, and carbonizing in an inert atmosphere to obtain a C / Si precursor; the organic acid comprises at least one of oxalic acid, tannic acid, acetic acid, and citric acid;

[0010] Removing the silicon template and recovering the silicon source: treating the C / Si precursor with hydrofluoric acid, and obtaining mesoporous carbon and fluorosilicic acid solution by solid-liquid separation. The fluorosilicic acid solution is used to prepare the silicon template.

[0011] The process of the present invention is based on the hard template method to prepare mesoporous carbon. Fluorosilicic acid is used as a silicon source to react with calcium carbonate to obtain a silica sol template. The carbon source and the silica sol template are mixed and carbonized to obtain a carbon / silicon precursor. The silicon template is removed by hydrofluoric acid to obtain the product mesoporous carbon. The generated acid waste liquid contains fluosilicic acid, which can be directly recycled as a silicon source and react with the next batch of calcium carbonate to obtain a silica sol template, thereby realizing silicon source recycling. The mesoporous carbon prepared by this process has the advantages of small pore size, large specific surface area, adjustable pore volume, etc., and basically no waste liquid is generated during the preparation process.

[0012] The mesoporous carbon preparation process may also include: the calcium fluoride precipitate reacts with sulfuric acid to generate hydrofluoric acid for treating the C / Si precursor. That is, the hydrogen fluoride used to remove the silicon template in the process of the present invention can be partially or completely recovered from the fluorine resource during the circulation process of the fluosilicic acid solution, and is obtained by hydrolyzing the calcium fluoride precipitate formed by the calcium carbonate reaction in sulfuric acid. In this way, the process of the present invention can simultaneously realize the recycling of silicon and fluorine, and only requires the addition of calcium carbonate, sulfuric acid, carbon source and organic acid.

[0013] The fluorosilicic acid solution used in the mesoporous carbon preparation process can be a byproduct of the fertilizer industry and / or recycled from fluorosilicic acid waste liquid after treating C / Si precursor with hydrofluoric acid.

[0014] In the mesoporous carbon preparation process, the silica sol obtained in the silicon template preparation process is an acidic silica sol with a pH of 2 to 5 and a silica concentration of 1 to 8 wt%. The silica morphology in the acidic silica sol is not fixed, and most of them are spherical silicon monomers and silicon oxygen oligomers with a particle size of about 7 nm, and their surfaces contain abundant silicon hydroxyl groups. After adjusting the pH to alkaline or drying, the oligomers and silicon monomers are polymerized to form closely arranged silica spheres of about 15 nm.

[0015] In the process of preparing the mesoporous carbon, during the preparation of the silicon template, the mass ratio of calcium carbonate to water in the reaction system can be 1:2-7, the amount of calcium carbonate is just sufficient or excessive relative to the amount of fluorosilicic acid, and further, the molar ratio of fluorosilicic acid to calcium carbonate can be 1:3-5.

[0016] In the mesoporous carbon preparation process, the carbon source may include at least one of glucose, sucrose, lactose, maltose, glycine, humic acid, and soluble starch.

[0017] In the process of preparing the mesoporous carbon, during the preparation of the precursor, the mass ratio of the carbon source to the silicon dioxide in the silica sol can be 2 to 9:1.

[0018] In the process of preparing the mesoporous carbon, during the preparation of the precursor, the molar ratio of the organic acid to the silicon dioxide in the silica sol can be 0.01 to 0.5:1.

[0019] In the mesoporous carbon preparation process, the inert atmosphere is a gas atmosphere that does not participate in the reaction, and specifically may include a nitrogen atmosphere and / or an argon or other rare gas atmosphere.

[0020] In the mesoporous carbon preparation process, the carbonization temperature can be 700-850° C. and the time can be 1-2 hours.

[0021] In the process of preparing mesoporous carbon, during the process of treating the C / Si precursor with hydrofluoric acid, the molar ratio of hydrofluoric acid to silicon dioxide in the C / Si precursor can be 5.5 to 8:1.

[0022] In the process of preparing mesoporous carbon, the C / Si precursor is treated with hydrofluoric acid for a treatment time of 12 to 24 hours.

[0023] In the process of preparing mesoporous carbon, during the process of treating the C / Si precursor with hydrofluoric acid, the hydrofluoric acid can be used to treat the C / Si precursor in the form of a hydrofluoric acid aqueous solution. Furthermore, the mass fraction of hydrofluoric acid in the hydrofluoric acid aqueous solution can be 8% to 15%.

[0024] The present invention also provides mesoporous carbon prepared by the mesoporous carbon preparation process. Further, the specific surface area of ​​the mesoporous carbon is greater than 800 m 2 / g, and the pore size is less than 6nm.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The hard template used in the process of the present invention is fresh acidic silica sol obtained by the reaction of fluorosilicic acid and carbonate. The pH of fresh acidic silica sol is 2-5. The morphology of silica therein is not fixed. Most of them are spherical silicon monomers and silicon oxygen oligomers with a particle size of about 7nm, and their surfaces contain abundant silicon hydroxyl groups. Fresh acidic silica sol is directly added with soluble carbon source and organic acid without treatment; the surface functional groups of carbon source condense with silicon hydroxyl groups on the surface of silica, and the polymerization growth of silicon oxygen oligomers and silicon monomers is restricted during the drying and carbonization process, and the shrinkage of silica particles is promoted, so that the particle size of silica particles in C / Si composite is less than 6nm. The pore size of mesoporous carbon formed after silicon removal from C / Si composite obtained by this in-situ condensation and organic acid-assisted pore formation method is less than 6nm.

[0027] The mesoporous carbon prepared by the process of the present invention has high specific surface area, large pore volume, small pore size and uniform distribution, and basically no waste acid and waste alkali liquid is discharged during the preparation process of the process, and the obtained fluorosilicic acid solution can be recycled.

[0028] The process of the present invention is expected to provide ideas for the problem of waste liquid treatment during the large-scale production of mesoporous carbon; and the obtained mesoporous carbon with small pore size and large specific surface area has broad application prospects in the fields of catalysis, energy, adsorption, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The figure is a schematic diagram of the process for preparing mesoporous carbon with recyclable silicon source according to the present invention.

[0030] Figure 2 This is the N2 physical adsorption isotherm and pore size distribution diagram of the mesoporous carbon prepared in Example 3.

[0031] Figure 3 This is the N2 physical adsorption isotherm and pore size distribution diagram of the mesoporous carbon prepared in Example 8. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0033] An exemplary process for preparing mesoporous carbon with recyclable silicon source is shown in Figure 1 , which may include:

[0034] Preparation of silicon template: Fluorosilicic acid solution reacts with calcium carbonate, and calcium fluoride solid and silica sol are separated by filtration; calcium fluoride solid can be reacted with sulfuric acid to form hydrofluoric acid for removing silicon template;

[0035] Preparing the precursor: dissolving the carbon source and the organic acid in the silica sol to form a silicon-carbon composite precursor, drying, grinding, and carbonizing in an inert atmosphere to obtain a C / Si precursor (or silicon / carbon composite material);

[0036] Removing the silicon template and recovering the silicon source: After the C / Si precursor is crushed, it is soaked in hydrofluoric acid to remove silicon, and the solid-liquid separation is performed to obtain a mesoporous carbon solid and a dilute fluorosilicic acid solution. The dilute fluorosilicic acid solution can be concentrated to form a fluorosilicic acid solution for preparing the silicon template.

[0037] Example 1

[0038] (1) First, 7.5 g of calcium carbonate was added to 15 g of water in a mass ratio of 1:2. After mixing, 11.3 g of 30 wt% fluorosilicic acid solution was added. A large number of bubbles were generated during the reaction. After filtration, the filter cake was a mixture of calcium carbonate and calcium fluoride. The filtrate was a silica sol with a pH of 3.5 and a silicon dioxide concentration of 5.8 wt%.

[0039] (2) Add 3 g of glucose and 0.45 g of oxalic acid to the silica sol, dry at 110 °C for 6 h, grind the resulting block solid into powder, and program the temperature to 700 °C under a nitrogen atmosphere and maintain for 1 h to obtain a C / Si precursor.

[0040] (3) The C / Si precursor was added to 24 g of a 10 wt% hydrofluoric acid aqueous solution, allowed to stand for 12 h, and filtered to recover silicon from the filtrate. The filter cake was the mesoporous carbon product.

[0041] (4) Add 6 g of calcium carbonate to the filtrate to obtain silica sol again, completing the silicon cycle.

[0042] Example 2

[0043] (1) First, 7 g of calcium carbonate was added to 35 g of water in a mass ratio of 1:5. After mixing, 8 g of 30 wt% fluorosilicic acid solution was added and filtered. The filter cake was a mixture of calcium carbonate and calcium fluoride, and the filtrate was a silica sol with a pH of 3.4 and a silicon dioxide concentration of 2.4 wt%.

[0044] (2) Add 2.5 g of sucrose and 3 g of tannic acid to the silica sol, dry at 110 °C for 12 h, grind the resulting block solid into powder, and program the temperature to 850 °C under a nitrogen atmosphere and maintain for 1.5 h to obtain a C / Si precursor.

[0045] (3) The C / Si precursor was added to 22 g of a 10 wt% hydrofluoric acid aqueous solution, allowed to stand for 12 h, and filtered to recover silicon from the filtrate. The filter cake was the mesoporous carbon product.

[0046] (4) Add 7 g of calcium carbonate to the filtrate to obtain silica sol again, completing the silicon cycle.

[0047] Example 3

[0048] (1) First, 5 g of calcium carbonate was added to 15 g of water in a mass ratio of 1:3. After mixing, 8 g of 30 wt% fluorosilicic acid solution was added and filtered. The filter cake was calcium fluoride and the filtrate was a silica sol with a pH of 2.7 and a silicon dioxide concentration of 4.6 wt%.

[0049] (2) Add 8 g of sucrose and 0.3 g of oxalic acid to the silica sol, dry at 110 °C for 3 h and then at 160 °C for 3 h, grind the resulting solid block into powder, and heat the mixture to 800 °C in a nitrogen atmosphere and hold for 1 h to obtain a C / Si precursor.

[0050] (3) The C / Si precursor was added to 23 g of a 10 wt% hydrofluoric acid aqueous solution, allowed to stand for 18 h, and filtered. The filtrate was used to recover silicon, and the filter cake was the mesoporous carbon product.

[0051] (4) Add 5 g of calcium carbonate to the filtrate to obtain silica sol again, completing the silicon cycle.

[0052] Figure 2 N2 physical adsorption isotherm and pore size distribution diagram of the mesoporous carbon product prepared in this example.

[0053] Example 4

[0054] (1) First, 11.2 g of calcium carbonate was added to 33.6 g of water in a mass ratio of 1:3. After mixing, 19 g of 25 wt% fluorosilicic acid solution was added and filtered. The filter cake was a mixture of calcium carbonate and calcium fluoride, and the filtrate was a silica sol with a pH of 3.2 and a silicon dioxide concentration of 4.0 wt%.

[0055] (2) Add 10 g of soluble starch and 0.6 g of citric acid to the silica sol, dry at 110° C. for 12 h, grind the resulting block solid into powder, and program the temperature to 750° C. under a nitrogen atmosphere and maintain for 1.5 h to obtain a C / Si precursor.

[0056] (3) The C / Si precursor was added to 40 g of 8 wt % hydrofluoric acid aqueous solution, allowed to stand for 24 h, and filtered to recover silicon from the filtrate. The filter cake was the mesoporous carbon product.

[0057] (4) 8.4 g of calcium carbonate is added to the filtrate to obtain silica sol again, completing the silicon cycle.

[0058] Example 5

[0059] (1) First, 50 g of calcium carbonate was added to 100 g of water in a mass ratio of 1:2. After mixing, 70 g of 35 wt% fluorosilicic acid solution was added and filtered. The filter cake was calcium fluoride and the filtrate was a silica sol with a pH of 2.3 and a silicon dioxide concentration of 7.0 wt%.

[0060] (2) Add 40 g of glucose and 10.6 g of citric acid to the silica sol, dry at 160 °C for 12 h, grind the resulting block solid into powder, and program the temperature to 850 °C under a nitrogen atmosphere and maintain for 2 h to obtain a C / Si precursor.

[0061] (3) The C / Si precursor was added to 200 g of a 10 wt% hydrofluoric acid aqueous solution, allowed to stand for 24 h, and filtered to recover silicon from the filtrate. The filter cake was the mesoporous carbon product.

[0062] (4) Add 50 g of calcium carbonate to the filtrate to obtain silica sol again, completing the silicon cycle.

[0063] Example 6

[0064] (1) First, 11.6 g of calcium carbonate was added to 34.8 g of water in a mass ratio of 1:3. After mixing, 16 g of 30 wt% fluorosilicic acid solution was added and filtered. The filter cake was a mixture of calcium carbonate and calcium fluoride, and the filtrate was a silica sol with a pH of 2.7 and a silicon dioxide concentration of 4.2 wt%.

[0065] (2) Add 4 g of sucrose and 0.8 g of oxalic acid to the silica sol, dry at 110° C. for 12 h, grind the resulting block solid into powder, and program the temperature to 700° C. in a nitrogen atmosphere and maintain for 1 h to obtain a C / Si precursor.

[0066] (3) The C / Si precursor was added to 40 g of a 10 wt% hydrofluoric acid aqueous solution, allowed to stand for 12 h, and filtered to recover silicon from the filtrate. The filter cake was the mesoporous carbon product.

[0067] (4) 11.6 g of calcium carbonate is added to the filtrate to obtain silica sol again, completing the silicon cycle.

[0068] Example 7

[0069] (1) First, 5.1 g of calcium carbonate was added to 25.5 g of water in a mass ratio of 1:5. After mixing, 8 g of 30 wt% fluorosilicic acid solution was added and filtered. The filter cake was a mixture of calcium carbonate and calcium fluoride, and the filtrate was a silica sol with a pH of 2.9 and a silicon dioxide concentration of 3.1 wt%.

[0070] (2) Add 4 g of soluble starch and 0.5 g of tannic acid to the silica sol, dry at 110° C. for 6 h, grind the resulting block solid into powder, and program the temperature to 700° C. under an argon atmosphere and maintain for 1 h to obtain a C / Si precursor.

[0071] (3) The C / Si precursor was added to 25 g of 8 wt % hydrofluoric acid aqueous solution, allowed to stand for 12 h, and filtered. The filtrate was used to recover silicon, and the filter cake was the mesoporous carbon product.

[0072] (4) Add 6 g of calcium carbonate to the filtrate to obtain silica sol again, completing the silicon cycle.

[0073] Example 8

[0074] (1) First, 5.5 g of calcium carbonate was added to 11 g of water in a mass ratio of 1:2. After mixing, 12 g of 20 wt% fluorosilicic acid solution was added and filtered. The filter cake was a mixture of calcium carbonate and calcium fluoride, and the filtrate was a silica sol with a pH of 3.5 and a silicon dioxide concentration of 4.6 wt%.

[0075] (2) Add 2 g of sucrose and 0.3 g of oxalic acid to the silica sol, dry at 110 °C for 4 h and then at 160 °C for 4 h, grind the resulting solid block into powder, and heat the mixture to 800 °C in an argon atmosphere and hold for 1 h to obtain a C / Si precursor.

[0076] (3) The C / Si precursor was added to 24 g of a 10 wt% hydrofluoric acid aqueous solution, allowed to stand for 24 h, and filtered to recover silicon from the filtrate. The filter cake was the mesoporous carbon product.

[0077] (4) Add 6 g of calcium carbonate to the filtrate to obtain silica sol again, completing the silicon cycle.

[0078] Figure 3 N2 physical adsorption isotherm and pore size distribution diagram of the mesoporous carbon product prepared in this example.

[0079] Example 9

[0080] (1) First, 5 g of calcium carbonate was added to 15 g of water in a mass ratio of 1:3. After mixing, 8 g of 30 wt% fluorosilicic acid solution was added and filtered. The filter cake was calcium fluoride and the filtrate was a silica sol with a pH of 2.7 and a silicon dioxide concentration of 4.6 wt%.

[0081] (2) Add 8 g of sucrose and 0.3 g of oxalic acid to the silica sol, dry at 110 °C for 3 h and then at 160 °C for 3 h, grind the resulting solid block into powder, and heat the mixture to 800 °C in a nitrogen atmosphere and hold for 1 h to obtain a C / Si precursor.

[0082] (3) The calcium fluoride obtained in step 1 is added to a dilute sulfuric acid solution, heated at 70°C, and filtered to obtain a hydrofluoric acid solution and a calcium sulfate precipitate. The hydrofluoric acid solution is diluted to obtain 19 g of 10 wt% hydrofluoric acid, with a recovery rate of 95%.

[0083] (4) Add the C / Si precursor to the hydrofluoric acid obtained in step 3, let stand for 18 hours, filter, and recover silicon from the filtrate. The filter cake is the mesoporous carbon product.

[0084] (5) Add 5 g of calcium carbonate to the filtrate to obtain silica sol again, completing the silicon cycle.

[0085] Example 10

[0086] (1) First, 5.6 g of calcium carbonate was added to 16.8 g of water in a mass ratio of 1:3. After mixing, 12 g of 20 wt% fluorosilicic acid solution was added and filtered. The filter cake was a mixture of calcium carbonate and calcium fluoride, and the filtrate was a silica sol with a pH of 3.5 and a silicon dioxide concentration of 3.6 wt%.

[0087] (2) Add 5 g of soluble starch and 0.5 g of oxalic acid to the silica sol, dry at 110 °C for 6 h, grind the resulting block solid into powder, and program the temperature to 750 °C under a nitrogen atmosphere and maintain for 1.5 h to obtain a C / Si precursor.

[0088] (3) The C / Si precursor was added to 35 g of 8 wt % hydrofluoric acid aqueous solution, allowed to stand for 24 h, and filtered. The filtrate was used to recover silicon, and the filter cake was the mesoporous carbon product.

[0089] (4) 8.4 g of calcium carbonate is added to the filtrate to obtain silica sol again, completing the silicon cycle.

[0090] Embodiment 11

[0091] (1) First, 5.5 g of calcium carbonate was added to 11 g of water in a mass ratio of 1:2. After mixing, 24 g of 10 wt% fluorosilicic acid solution was added and filtered. The filter cake was a mixture of calcium carbonate and calcium fluoride, and the filtrate was a silica sol with a pH of 4.1 and a silicon dioxide concentration of 3.0 wt%.

[0092] (2) Add 4 g of sucrose and 0.2 g of acetic acid to the silica sol, dry at 110° C. for 8 h, grind the resulting block solid into powder, and program the temperature to 800° C. under a nitrogen atmosphere and maintain for 1.5 h to obtain a C / Si precursor.

[0093] (3) The C / Si precursor was added to 30 g of a 12 wt% hydrofluoric acid aqueous solution, allowed to stand for 24 h, and filtered to recover silicon from the filtrate. The filter cake was the mesoporous carbon product.

[0094] (4) Add 5.5 g of calcium carbonate to the filtrate to obtain silica sol again, completing the silicon cycle.

[0095] Comparative Example 1

[0096] The difference from Example 3 is that the silicon template used is commercially available silicon dioxide powder, and there is no silicon recycling.

[0097] (1) Weigh 2 g of commercially available silicon dioxide powder with a particle size of 15 nm and dissolve it in 30 g of water to form a suspension. Add 16 g of sucrose and 0.6 g of oxalic acid to dissolve it completely.

[0098] (2) The solution was dried at 110° C. for 3 h and then at 160° C. for 3 h to obtain a block solid, which was ground and heated to 800° C. in a nitrogen atmosphere and maintained for 1 h to obtain a C / Si precursor.

[0099] (3) The C / Si precursor was added to 20 g of a 10 wt% hydrofluoric acid aqueous solution, allowed to stand for 18 h, and filtered. The filter cake was the mesoporous carbon product.

[0100] Comparative Example 2

[0101] The difference from Example 8 is that the silicon template used is commercially available silicon dioxide powder, and there is no silicon recycling.

[0102] (1) Weigh 1 g of commercially available silicon dioxide powder with a particle size of 15 nm and dissolve it in 16 g of water to form a suspension. Add 2 g of sucrose and 0.3 g of oxalic acid to dissolve it completely.

[0103] (2) The solution was dried at 110° C. for 4 h and at 160° C. for 4 h to obtain a block solid, which was ground and heated to 800° C. in an argon atmosphere and maintained for 1 h to obtain a C / Si precursor.

[0104] (3) The C / Si precursor was added to 20 g of a 10 wt% hydrofluoric acid aqueous solution, allowed to stand for 24 h, and filtered. The filter cake was the mesoporous carbon product.

[0105] Comparative Example 3

[0106] (1) First, 5 g of calcium carbonate was added to 15 g of water in a mass ratio of 1:3. After mixing, 8 g of 30 wt% fluorosilicic acid solution was added and filtered. The filter cake was calcium fluoride and the filtrate was silica sol.

[0107] (2) The pH value of the silica sol is adjusted to 6-8, the silica sol is rapidly gelled and precipitated, and then dried and ground to obtain silicon dioxide powder.

[0108] (3) Add silica powder to 21 g of water, mix well, then add 8 g of sucrose and 0.3 g of oxalic acid; dry at 110° C. for 3 h and then at 160° C. for 3 h, grind the resulting solid block into powder, and heat to 800° C. in a nitrogen atmosphere and hold for 1 h to obtain a C / Si precursor.

[0109] (3) The C / Si precursor was added to 23 g of a 10 wt% hydrofluoric acid aqueous solution, allowed to stand for 18 h, and filtered. The filtrate was used to recover silicon, and the filter cake was the mesoporous carbon product.

[0110] (4) Add 5 g of calcium carbonate to the filtrate to obtain silica sol again, completing the silicon cycle.

[0111] Comparative Example 4

[0112] The only difference from Example 3 is that after the silica sol is prepared in step (1), its pH is adjusted to 12-13 with aqueous ammonia. In this process, the silica sol is still in the form of a sol and no gel precipitation occurs.

[0113] Comparative Example 5

[0114] (1) Take 10g of calcium carbonate and add it to 10g of water. After mixing, add 10g of 40wt% fluorosilicic acid solution and filter. The filter cake is calcium fluoride and the filtrate is 9.4wt% silica sol.

[0115] (2) Add 16 g of sucrose and 0.3 g of oxalic acid to the silica sol, dry at 110 °C for 3 h and then at 160 °C for 3 h, grind the resulting solid block into powder, and heat the mixture to 800 °C in a nitrogen atmosphere and hold for 1 h to obtain a C / Si precursor.

[0116] (3) The C / Si precursor was added to 23 g of a 10 wt% hydrofluoric acid aqueous solution, allowed to stand for 18 h, and filtered. The filtrate was used to recover silicon, and the filter cake was the mesoporous carbon product.

[0117] (4) Add 5 g of calcium carbonate to the filtrate to obtain silica sol again, completing the silicon cycle.

[0118] Comparative Example 6

[0119] The only difference from Example 8 is that no organic acid is added during the preparation of the precursor in step 2, and the rest is the same.

[0120] Comparative Example 7

[0121] (1) Take 2 g of ordered mesoporous silica SBA-15 and add it to 21 g of water, then add 4 g of sucrose and 0.6 g of oxalic acid, mix well and dry at 110 ° C for 4 h, then dry at 160 ° C for 4 h, grind the obtained block solid into powder, and heat it to 800 ° C in an argon atmosphere and keep it for 1 h to obtain a C / Si precursor.

[0122] (2) The C / Si precursor was added to 24 g of a 10 wt% hydrofluoric acid aqueous solution, allowed to stand for 24 h, and filtered. The filtrate was a fluorosilicic acid solution, and the filter cake was a mesoporous carbon product.

[0123] Comparative Example 8

[0124] The only difference from Comparative Example 7 is that the solution used for desiliconization of the C / Si precursor is a 1.3 mol / L sodium hydroxide ethanol aqueous solution, wherein the mass ratio of ethanol to water is 2: 1. The filtrate obtained in this comparative example is an ethanol aqueous solution of sodium silicate.

[0125] Table 1 shows the physical properties, carbonization yield and silicon recovery rate of the mesoporous carbon products prepared by the processes of various embodiments.

[0126] Table 1

[0127]

[0128] The carbonization yield is the mass of mesoporous carbon product / the mass of added carbon source × 100%;

[0129] The silicon recovery rate is the number of moles of silicon in the filtrate fluosilicic acid / the raw fluosilicic acid solution×100%.

[0130] Table 2 shows the physical properties, carbonization yield and silicon recovery rate of the mesoporous carbon products prepared by the comparative examples.

[0131] Table 2

[0132]

[0133] The carbonization yield is the mass of mesoporous carbon product / the mass of added carbon source × 100%;

[0134] The silicon recovery rate is the number of moles of silicon in the filtrate fluosilicic acid / the raw material fluosilicic acid solution×100%.

[0135] Comparing Example 3 with Comparative Example 1, it can be found that under the same conditions, the prepared mesoporous carbon with a smaller particle size of 2.5 nm and a larger specific surface area of ​​863 m 2 / g.

[0136] By comparing Example 8 with Example 3, it can be found that after reducing the mass ratio of carbon source to silica sol, the specific surface area and pore volume of the prepared mesoporous carbon increased significantly, and the pore diameter was still below 6nm. This is because after reducing the mass ratio of carbon source to silica sol, the carbon source condensed on the surface of silica sol is reduced, and the confinement effect of carbon source on silicon-oxygen monomers and silicon-oxygen oligomers is weakened during the drying and carbonization process, and the reduction of carbon source leads to the thinning of the carbon layer in the C / Si composite after carbonization; accordingly, the pore volume, pore diameter, and specific surface area of ​​the mesoporous carbon in the product increase to varying degrees.

[0137] By comparing Example 8 with Comparative Example 2, it can be found that after changing the mass ratio of carbon source to silica sol, the mesoporous carbon prepared by the same method using commercially available silica powder with a particle size of about 15 nm as a template has a small increase in specific surface area and pore volume, and the pore size remains basically unchanged. It is easier to adjust the properties of mesoporous carbon by using the silica sol of the present invention as a template to prepare mesoporous carbon.

[0138] By comparing Example 9 with Example 3, it can be found that the properties and silicon recovery rate of the mesoporous carbon samples obtained by recovering hydrofluoric acid with calcium fluoride and adding hydrofluoric acid as the silicon removal solution are basically the same, which proves that the fluorine resource recycling in this method is feasible.

[0139] By comparing Example 3 with Comparative Examples 3 and 4, it can be found that when the properties of the acidic silica sol are changed and the mesoporous carbon is prepared by the same method using alkaline silica sol or silica powder after gel as a template, the specific surface area and pore volume of the mesoporous carbon are significantly reduced, and the pore size is significantly increased. This is because after the pH of the solution is changed to neutral or alkaline without the confinement of the carbon source, the silicon monomers and silicon oxygen oligomers in the original acidic silica sol polymerize into small spheres with a particle size of about 15nm, which are similar to the properties of commercially available silica with a particle size of about 15nm; accordingly, the properties of the mesoporous carbon prepared using the two as templates are also similar.

[0140] Comparing Example 3 with Comparative Example 5, it can be found that under the same conditions, the pore size of the mesoporous carbon prepared with high concentration silica sol as a template increases, while the specific surface area and pore volume decrease; similar to the effect brought about by adjusting the pH of the silica sol, when the concentration of the silica sol is too high, the silicon monomers and silicon oxygen oligomers inside it spontaneously polymerize to form spherical silica particles, and the particle size of the silica particles that act as a template during the dehydration and carbonization process becomes larger; accordingly, the pore size of the mesoporous carbon product increases, the pore volume decreases, and the specific surface area decreases.

[0141] By comparing Example 8 with Comparative Example 6, it can be found that in the process of preparing the precursor, if no organic acid is added to assist in pore formation, the pore size of the obtained mesoporous carbon increases significantly, and the specific surface area and pore volume decrease significantly; this is because the organic acid accelerates the condensation of hydroxyl groups during the dissolution of the carbon source in the silica sol, making the pre-oxidation process of the carbon source before carbonization more complete, intensifying the shrinkage of silica during the dehydration of the silica sol, and assisting the carbonization process of the carbon source; and the organic acid decomposes at high temperature to produce gas to assist in pore formation, increasing the specific surface area and pore volume. If oxalic acid is not added, the carbonization yield of the mesoporous carbon product decreases, the pore size becomes larger, and accordingly, its specific surface area and pore volume decrease.

[0142] By comparing Example 8 with Comparative Examples 7 and 8, it can be found that mesoporous carbon with a pore size of less than 6 nm can be obtained by using ordered mesoporous silica SBA-15 as a template; however, the waste liquid generated by this method for removing silicon is fluorosilicic acid or sodium silicate solution, and it is difficult to re-prepare the template SBA-15 with the two waste liquids. The pore size of the mesoporous carbon prepared by this method can be maintained at 2 to 6 nm, and the preparation process realizes the silicon template cycle, and basically no waste liquid is generated.

[0143] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A process for preparing mesoporous carbon with recyclable silicon source, characterized in that: include: Preparation of silicon template: Fluorosilicic acid solution reacts with calcium carbonate to separate calcium fluoride precipitate and silica sol; the pH of the silica sol is 2 to 5; the concentration of silicon dioxide in the silica sol is 1 to 8 wt%; Preparing a precursor: dissolving a carbon source and an organic acid in a silica sol, drying, grinding, and carbonizing in an inert atmosphere to obtain a C / Si precursor; the organic acid comprises at least one of oxalic acid, tannic acid, acetic acid, and citric acid; Removing the silicon template and recovering the silicon source: treating the C / Si precursor with hydrofluoric acid, and obtaining mesoporous carbon and fluorosilicic acid solution by solid-liquid separation. The fluorosilicic acid solution is used to prepare the silicon template.

2. The process for preparing mesoporous carbon according to claim 1, characterized in that: The mesoporous carbon preparation process also includes: the calcium fluoride precipitate reacts with sulfuric acid to generate hydrofluoric acid for treating the C / Si precursor.

3. The process for preparing mesoporous carbon according to claim 1, characterized in that: The fluorosilicic acid solution used in the mesoporous carbon preparation process is a byproduct of the fertilizer industry and / or is obtained by recycling fluorosilicic acid waste liquid after treating C / Si precursor with hydrofluoric acid.

4. The process for preparing mesoporous carbon according to claim 1, characterized in that: During the preparation of the silicon template, the mass ratio of calcium carbonate to water in the reaction system is 1:2-7, the amount of calcium carbonate is just sufficient or excessive relative to the amount of fluorosilicic acid, and further, the molar ratio of fluorosilicic acid to calcium carbonate is 1:3-5.

5. The process for preparing mesoporous carbon according to claim 1, characterized in that: The carbon source includes at least one of glucose, sucrose, lactose, maltose, glycine, humic acid and soluble starch.

6. The process for preparing mesoporous carbon according to claim 1, characterized in that: During the preparation of the precursor, the mass ratio of the carbon source to the silicon dioxide in the silica sol is 2 to 9:

1.

7. The process for preparing mesoporous carbon according to claim 1, characterized in that: In the process of preparing the precursor, the molar ratio of the organic acid to the silicon dioxide in the silica sol is 0.01 to 0.5:

1.

8. The process for preparing mesoporous carbon according to claim 1, characterized in that: The inert atmosphere is a nitrogen atmosphere and / or a rare gas atmosphere; The carbonization temperature is 700-850° C. and the time is 1-2 hours.

9. The process for preparing mesoporous carbon according to claim 1, characterized in that: During the treatment of C / Si precursor with hydrofluoric acid: The molar ratio of hydrofluoric acid to silicon dioxide in the C / Si precursor is 5.5 to 8:1; The processing time is 12 to 24 hours; In the process of treating the C / Si precursor with hydrofluoric acid, the hydrofluoric acid treats the C / Si precursor in the form of a hydrofluoric acid aqueous solution, and the mass fraction of the hydrofluoric acid in the hydrofluoric acid aqueous solution is 8% to 15%.

10. The mesoporous carbon prepared by the process for preparing mesoporous carbon according to any one of claims 1 to 9, characterized in that: The specific surface area of ​​the mesoporous carbon is greater than 800 m 2 / g, and the pore size is less than 6nm.

Citation Information

Patent Citations

  • Method for preparing acrylonitrile polymer based mesoporous carbon

    CN101696005A

  • Alkaline mesoporous carbon catalyst for room-temperature oxidation of H2S, preparation method and application

    CN108014835A

  • Method for preparing high-purity fluorite through rapid reaction of fluosilicic acid and calcium carbonate

    CN111533152A

  • Method for preparing porous carbon and white carbon black by using diatomite

    CN101913595A

  • Preparation method of foaming ordered mesoporous carbon integral material with graded tunnel structure

    CN102249213A