Preparation method of negative electrode material, negative electrode material prepared by negative electrode material and lithium ion battery containing negative electrode material
The high-pressure sol-gel method is used to treat natural graphite to form densified spherical graphite colloids, which solves the internal defects and void problems of natural graphite, significantly improves its circulation and rate performance, achieves performance comparable to artificial graphite, and reduces the Production cost.
Patent Information
- Application Number
- CN202411166766.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-08
AI Technical Summary
There are large defects and voids inside the natural graphite negative electrode material, resulting in poor cycle performance, magnification and kinetic performance deviations. The existing modification methods are costly or complex in process, and cannot effectively improve the pore structure.
The high-pressure sol-gel method is adopted to form a densified spherical graphite colloid through hydrogen fluoride solution treatment and resorcinol-formaldehyde resin sol-gel method, and the densified spherical graphite colloid is cured and crosslinked under high temperature and high pressure to fill the internal defects of natural graphite. Improve conductivity and consistency.
It significantly improves the circulation, magnification and kinetic properties of natural graphite, making its performance close to artificial graphite, and has a simple process, suitable for industrial production, and has a high overall cost-effectiveness.
Smart Images

Figure CN118908201A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials, and specifically discloses a negative electrode material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are one of the most common types of batteries currently used in electric vehicles, portable electronic devices, and energy storage systems. They are widely used because of their high energy density, long cycle life, low self-discharge rate, and environmental friendliness. Lithium-ion batteries consist of a positive electrode, a negative electrode, an electrolyte, and a separator, of which the negative electrode is an important component of the battery and has an important influence on battery performance, capacity, rate, cycle stability, safety, and other properties.
[0003] The advantages of natural graphite as a negative electrode material are low price, low energy consumption, and low environmental pollution. However, at present, natural graphite is made of flake graphite as raw material, and spherical graphite of different particle sizes is obtained through coarse crushing, shaping and grading. The process of spherical graphite formation is that the flake graphite layers are gradually bent, folded and sphericalized under external forces. Its formation process determines that there are large defects and gaps inside the negative electrode spherical natural graphite. These congenital defects cause poor compatibility with the electrolyte, increased side reactions, and poor overall cycle performance when used as the negative electrode of lithium-ion batteries. Its preparation process and high degree of graphitization also determine that the graphite interlayer spacing of natural graphite is small and the electronic conductivity performance is biased, resulting in poor kinetic performance and poor rate performance. The above-mentioned shortcomings of natural graphite limit its large-scale application in the fields of power and energy storage.
[0004] CN111320171A discloses a low-expansion graphite negative electrode material, a preparation method thereof, and a lithium-ion battery. The preparation method comprises (1) mixing a graphite raw material with a modifier and heating the mixture to obtain modified graphite; (2) heat-treating the modified graphite under a protective atmosphere to obtain heat-treated graphite; (3) post-treating the heat-treated graphite to obtain the graphite negative electrode material. The natural graphite modification method has the disadvantages of low sphericity, high expansion rate, and poor dynamics in battery applications.
[0005] CN114843508A discloses a modified natural graphite material and a preparation method thereof, a negative electrode plate and a lithium ion battery. The modified natural graphite material comprises a natural graphite matrix; non-graphitized carbon, at least part of the pores in the natural graphite matrix are filled with the non-graphitized carbon; the pore volume of the modified natural graphite material is 0.004 cm 3 / g~0.009cm 3 / g. The modified natural graphite prepared by this method has the disadvantages of high impurities, poor material consistency, complex process and high cost, no obvious improvement in product kinetic performance and deviation in product rate performance.
[0006] At present, the modification of existing natural graphite mainly involves modifying surface defects by coating the solid surface with amorphous carbon. Although surface defects can be modified to a certain extent and the conductivity and cycle stability of natural graphite can be improved, it cannot effectively improve the pore structure inside the natural graphite particles. This leads to the occurrence of side reactions during the cycle, which in turn causes the expansion rate of natural graphite negative electrode materials to increase and the cycle performance to decrease.
[0007] There are two main ways to optimize and improve the internal pore structure of natural graphite. One is to perform high-temperature graphitization on spherical graphite, and heat it at 2800-3000℃ to change its structure, so as to obtain highly crystallized and densely arranged spherical natural graphite. However, the cost of high-temperature graphitization is relatively high. Although the performance of natural graphite improved by densification through graphitization has been improved to a certain extent, its cost advantage has completely disappeared, and the overall cost performance is low. Another way to optimize the internal pores is to use the impregnation method, using one or two or more of carbon-containing organic matter including petroleum asphalt, coal asphalt, mesophase asphalt, phenolic resin, epoxy resin, coal tar and heavy oil to enter the interior of natural graphite through impregnation, and then convert it into amorphous carbon through high-temperature graphitization, so as to fill the internal pore defects of natural graphite. This type of method is complicated to operate and the impregnation effect is generally biased, resulting in poor product consistency and no obvious improvement in product performance. Summary of the invention
[0008] Technical issues One purpose of the present invention is to solve the problem of large defects and voids inside natural graphite negative electrode materials, as well as the resulting poor overall cycle performance, rate and kinetic performance deviations. The present invention adopts a high-pressure sol-gel method to achieve the preparation of densified natural graphite, thereby improving the cycle, rate, kinetics and other comprehensive performances of the natural graphite negative electrode, making its performance equivalent to that of artificial graphite as a whole. In addition, the present invention is combined with the existing spherical natural graphite negative electrode production process, suitable for industrial production, and has a high comprehensive cost performance.
[0009] Technical Solution In order to solve the above technical problems, the present invention provides a method for preparing a negative electrode material, comprising the following steps: S1. Sieving and classifying natural flake graphite powder to obtain raw materials; S2, adding the above raw materials to an aqueous solution of hydrogen fluoride and stirring, then filtering and washing to obtain a primary purified modified graphite; then adding the above primary purified modified graphite to an ethanol aqueous solution of hydrogen fluoride and continuing to stir to obtain a suspension; S3, adding resorcinol and formaldehyde to the suspension under stirring, and continuing stirring to obtain a graphite sol; S4, placing the graphite sol in a liquid phase spheroidizing shaping machine, shaping it in a sol state to obtain a spherical graphite colloid; S5, curing and cross-linking the spherical graphite colloid under high temperature and high pressure to obtain a gel; S6, centrifuging the gel to separate the solid product, washing with a mixture of water and ethanol until neutral (pH=7), and drying to obtain gel-filled natural graphite spheres; S7. Carbonizing the above-mentioned gel-filled natural graphite spheres under the protection of an inert atmosphere to obtain modified natural graphite microspheres, and obtaining negative electrode materials after demagnetization and screening.
[0010] Since the flake graphite raw material is treated with hydrogen fluoride solution, the acid washing purification of the raw material end can greatly improve the purification efficiency, and hydrofluoric acid has obvious impurity removal effect on metals such as Ca, Mg, Fe and their oxides; moreover, fluoride ion treatment can open the closed pores on the surface of flake graphite, and at the same time, surface fluorination improves the hydrophilicity of graphite, which is conducive to the densification of gel; thirdly, fluoride ions will fill in the inside of graphite, significantly improving the conductivity of the material; Among them, the sol-gel method is used to prepare resorcinol-formaldehyde (RF) resin. By using hydrofluoric acid to adjust the surface charge and then coordinating with the temperature, the degree of cross-linking can be precisely controlled; resorcinol has good chemical stability and can exist stably under acidic conditions; resorcinol has good high temperature resistance and mechanical wear resistance, and will not deteriorate or deform under high temperature and high pressure, and can improve the degree and efficiency of spherical graphitization in the liquid phase spheroidal graphite process; In step S5, a high-pressure sol-gel is prepared, and the filling of the cross-linked resin in the spherical graphite is further improved through mechanical pressure, thereby ensuring the densification and consistency of the product and improving the electronic conductivity and cycle performance of natural graphite.
[0011] According to one embodiment of the present invention, In step S1, the flake graphite is flaky crystalline graphite obtained by processing natural graphite ore, and the carbon content of the flake graphite is above 95%; The natural flake micro-powder graphite is passed through a 50-450 mesh sieve, and the sieve residue is taken to obtain a raw material.
[0012] According to one embodiment of the present invention, In step S2, the concentration of the aqueous hydrogen fluoride solution is 20-60 wt%, preferably 30-50 wt%, more preferably 40 wt%, the mass ratio of the raw material to the aqueous hydrogen fluoride solution is 1:(0.5-10), preferably 1:(1-5); the stirring speed is 30 rpm-1000 rpm; the stirring time is 20-60 min; The mass ratio of the primary purified modified graphite to the ethanol aqueous solution of hydrogen fluoride is 1: (0.2-5); preferably 1: (0.5-2); the stirring speed is 30rpm-1000rpm; the stirring time is 20-60 min; in the ethanol aqueous solution of hydrogen fluoride, the concentration of hydrogen fluoride is 20-60 wt%, preferably 30-50 wt%, and a mixture of ethanol and water is used as a solvent, and the weight ratio of ethanol to water is 1: (3-5).
[0013] According to one embodiment of the present invention, In step S3, resorcinol is added to the graphite suspension and stirred to obtain a resorcinol-graphite suspension, wherein the mass ratio of the graphite to the resorcinol is 1:(0.05-0.5), the stirring time is 15-60 min, and the stirring speed is 30 rpm-1000 rpm; Add formaldehyde to the above-obtained resorcinol graphite suspension and stir, wherein the molar ratio of resorcinol to formaldehyde is 1:(1-4); after the formaldehyde is completely added, stir continuously at 30-45° C. and 30 rpm-1000 rpm for 16-48 hours to obtain a graphite sol.
[0014] In a specific embodiment, the step of adding formaldehyde can be performed by adding it in small amounts multiple times.
[0015] According to one embodiment of the present invention, In step S5, curing is performed at a temperature of 70-200° C. and a pressure of 50-400 MPa for 10-120 min to obtain a gel.
[0016] According to one embodiment of the present invention, In step S6, centrifugal separation is performed at 6000-12000 rpm, washed with 30-70 wt % ethanol aqueous solution, and dried at 80-120° C. for 3-7 hours.
[0017] According to one embodiment of the present invention, In step S7, the inert atmosphere is nitrogen, the high temperature carbonization temperature is 1000-1300°C, and the carbonization time is 2-24h.
[0018] According to one aspect of the present invention, a negative electrode material prepared according to the above method is provided.
[0019] According to one aspect of the present invention, a lithium ion battery is provided, which comprises a negative electrode material prepared according to the above method.
[0020] Beneficial Effects The present invention adopts a high-pressure sol-gel method to form a core-shell graphite with internal densification and external RF-based coating. The method significantly improves the initial efficiency of natural graphite, improves the rate fast charging performance, improves the electronic conductivity performance, and has excellent cycle performance. In addition, the process of the present invention is simple, and the production line is consistent with the existing natural graphite negative electrode product production line, which is suitable for industrial production.
[0021] The flake graphite sol of the present invention is combined with liquid phase spheroidal graphite technology to improve the ball milling efficiency of the product. The product has a high degree of spheroidization and the internal sol is completely filled, which determines its high densification degree, improves the homogeneity of the product, reduces the pole piece layer expansion rate, and improves the product cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a SEM image of the modified natural graphite prepared according to Example 1 of the present invention. DETAILED DESCRIPTION
[0023] In order to enable persons with ordinary knowledge in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and the scope of the patent application. Unless otherwise specified, all technical and scientific words used in the text have the common meanings understood by those skilled in the art for the present invention. In case of conflict, the definitions in this specification shall prevail.
[0024] The following detailed description is merely illustrative in nature and is not intended to limit the present invention and its use. In addition, this document is not limited by any theory described in the above prior art or invention summary or the following detailed description or examples.
[0025] In the following examples, unless otherwise specified, the reagents used were all commercially available; the instruments used were all commonly used equipment in the industry.
[0026] Example Example 1 Method for preparing negative electrode material The natural flake micro powder graphite (200MESH) purchased from Qingdao Langrui Graphite Co., Ltd. was passed through a 200 mesh sieve to obtain the undersize; Then, the above-mentioned undersize (4KG) was added into a 40wt% hydrogen fluoride aqueous solution (10KG) and rapidly stirred (180rpm, 30min), and then filtered to obtain the primary purified modified graphite; Then, the above-mentioned primary purified modified graphite (4KG) was added into a 20% ethanol aqueous solution of hydrogen fluoride (4KG) and stirred continuously (stirring speed 600rpm, 30min) to obtain a suspension; wherein the weight ratio of ethanol to water was 1:4.
[0027] Add resorcinol (1.6 kg) to the graphite suspension, and then continue to stir at high speed for 30 minutes at a stirring speed of 300 rpm to obtain a resorcinol graphite suspension; Add 44 wt % formaldehyde aqueous solution (1.98 kg) in small amounts and repeatedly to the above-obtained resorcinol graphite suspension and continue stirring (300 rpm); after the formaldehyde is completely added, continue stirring at 300 rpm for 24 hours at 30° C. to obtain a graphite sol; Then the graphite sol is placed in a liquid phase ball mill and shaped in a sol state to obtain a spherical graphite colloid; Then, the spherical graphite colloid is placed in a mold, and cured and cross-linked for 60 minutes under high temperature and high pressure (120° C., 250 MPa pressure) to obtain a gel; Then, the gel solution was centrifuged (8000 rpm) to separate the solid product, which was washed with 50 wt % ethanol aqueous solution until the pH value was 7, and dried at 100 ° C for 5 h to obtain gel-filled natural graphite spheres; The gel-filled natural graphite spheres were carbonized at high temperature (1200°C for 14 h) under N2 protection to obtain modified natural graphite microspheres, which were then demagnetized and sieved to obtain the negative electrode product.
[0028] The obtained product was observed with a German ZEISS Zeiss Sigma300 instrument (1000x), and the Figure 1 The cross-sectional SEM images are shown.
[0029] Example 2 Method for preparing negative electrode material The natural flake micro powder graphite (200MESH) purchased from Qingdao Langrui Graphite Co., Ltd. was passed through a 200 mesh sieve to obtain the undersize; Then, the above-mentioned undersize (4KG) was added into a 40wt% hydrogen fluoride aqueous solution (10KG) and rapidly stirred (180rpm, 30min), and then filtered to obtain the primary purified modified graphite; Then, the above-mentioned primary purified modified graphite (4KG) was added into a 20% ethanol aqueous solution of hydrogen fluoride (4KG) and stirred continuously (stirring speed 600rpm, 30min) to obtain a suspension; wherein the weight ratio of ethanol to water was 1:3.
[0030] Add resorcinol (0.4 kg) to the graphite suspension, and then continue to stir at a high speed for 30 minutes at a stirring speed of 300 rpm to obtain a resorcinol graphite suspension; Add 44 wt % formaldehyde aqueous solution (0.495 kg) in small amounts and repeatedly to the above-obtained resorcinol graphite suspension and continue stirring (300 rpm); after the formaldehyde is completely added, continue stirring at 30° C. and 300 rpm for 24 hours to obtain a graphite sol; Then the graphite sol is placed in a liquid phase ball mill and shaped in a sol state to obtain a spherical graphite colloid; Then, the spherical graphite colloid is placed in a mold, and cured and cross-linked for 60 minutes under high temperature and high pressure (120° C., 250 MPa pressure) to obtain a gel; Then, the gel solution was centrifuged (8000 rpm) to separate the solid product, which was washed with 50 wt % ethanol aqueous solution until the pH value was 7, and dried at 100 ° C for 5 h to obtain gel-filled natural graphite spheres; The gel-filled natural graphite spheres were carbonized at high temperature (1200°C for 14 h) under N2 protection to obtain modified natural graphite microspheres, which were then demagnetized and sieved to obtain the negative electrode product.
[0031] Example 3 Method for preparing negative electrode material The natural flake micro powder graphite (200MESH) purchased from Qingdao Langrui Graphite Co., Ltd. was passed through a 200 mesh sieve to obtain the undersize; Then, the above-mentioned undersize (4KG) was added into a 40wt% hydrogen fluoride aqueous solution (10KG) and rapidly stirred (180rpm, 30min), and then filtered to obtain the primary purified modified graphite; Then, the above-mentioned primary purified modified graphite (4KG) was added into a 20% ethanol aqueous solution of hydrogen fluoride (4KG) and stirred continuously (stirring speed 600rpm, 30min) to obtain a suspension; wherein the weight ratio of ethanol to water was 1:4.
[0032] Add resorcinol (1.6 kg) to the graphite suspension, and then continue to stir at high speed for 30 minutes at a stirring speed of 300 rpm to obtain a resorcinol graphite suspension; Add 44 wt % formaldehyde aqueous solution (1.98 kg) in small amounts and repeatedly to the above-obtained resorcinol graphite suspension and continue stirring (300 rpm); after the formaldehyde is completely added, continue stirring at 300 rpm for 24 hours at 30° C. to obtain a graphite sol; Then the graphite sol is placed in a liquid phase ball mill and shaped in a sol state to obtain a spherical graphite colloid; Then, the spherical graphite colloid is placed in a mold, and cured and cross-linked for 60 minutes at high temperature and high pressure (80°C, 60MPa pressure) to obtain a gel; Then, the gel solution was centrifuged (8000 rpm) to separate the solid product, which was washed with 50 wt % ethanol aqueous solution until the pH value was 7, and dried at 100 ° C for 5 h to obtain gel-filled natural graphite spheres; The gel-filled natural graphite spheres were carbonized at high temperature (1200°C for 14 h) under N2 protection to obtain modified natural graphite microspheres, which were then demagnetized and sieved to obtain the negative electrode product.
[0033] Comparative Example 1 Conventional lithium-ion battery natural graphite single particle HG-15 purchased from Dalian Hongguang Lithium Industry Co., Ltd. was used as the negative electrode material of Comparative Example 1.
[0034] Comparative Example 2 Method for preparing negative electrode material The natural flake micro powder graphite (200MESH) purchased from Qingdao Langrui Graphite Co., Ltd. was passed through a 200 mesh sieve to obtain the undersize; Then, the above-mentioned undersize (4KG) was added into a 40wt% hydrogen fluoride aqueous solution (10KG) and rapidly stirred (180rpm, 30min), and then filtered to obtain the primary purified modified graphite; Then, the above-mentioned primary purified modified graphite (4KG) was added into a 20% ethanol aqueous solution of hydrogen fluoride (4KG) and stirred continuously (stirring speed 600rpm, 30min) to obtain a suspension; wherein the weight ratio of ethanol to water was 1:4.
[0035] Add resorcinol (0.16 kg) to the graphite suspension, and then continue to stir at a high speed for 30 minutes at a stirring speed of 300 rpm to obtain a resorcinol graphite suspension; Add 44 wt % formaldehyde aqueous solution (0.198 kg) in small amounts and repeatedly to the above-obtained resorcinol graphite suspension and continue stirring (300 rpm); after the formaldehyde is completely added, continue stirring at 30° C. and 300 rpm for 24 hours to obtain a graphite sol; Then the graphite sol is placed in a liquid phase ball mill and shaped in a sol state to obtain a spherical graphite colloid; Then, the spherical graphite colloid is placed in a mold, and cured and cross-linked for 60 minutes under high temperature and high pressure (120° C., 250 MPa pressure) to obtain a gel; Then, the gel solution was centrifuged (8000 rpm) to separate the solid product, which was washed with 50 wt % ethanol aqueous solution until the pH value was 7, and dried at 100 ° C for 5 h to obtain gel-filled natural graphite spheres; The gel-filled natural graphite spheres were carbonized at high temperature (1200°C for 14 h) under N2 protection to obtain modified natural graphite microspheres, which were then demagnetized and sieved to obtain the negative electrode product.
[0036] Comparative Example 3 Method for preparing negative electrode material The natural flake micro powder graphite (200MESH) purchased from Qingdao Langrui Graphite Co., Ltd. was passed through a 200 mesh sieve to obtain the undersize; Then, the above-mentioned undersize (4KG) was added into a 40wt% hydrogen fluoride aqueous solution (10KG) and rapidly stirred (180rpm, 30min), and then filtered to obtain the primary purified modified graphite; Then, the above-mentioned primary purified modified graphite (4KG) was added into a 20% ethanol aqueous solution of hydrogen fluoride (4KG) and stirred continuously (stirring speed 600rpm, 30min) to obtain a suspension; wherein the weight ratio of ethanol to water was 1:6.
[0037] Add resorcinol (1.6 kg) to the graphite suspension, and then continue to stir at high speed for 30 minutes at a stirring speed of 300 rpm to obtain a resorcinol graphite suspension; Add 44 wt % formaldehyde aqueous solution (1.98 kg) in small amounts and repeatedly to the above-obtained resorcinol graphite suspension and continue stirring (300 rpm); after the formaldehyde is completely added, continue stirring at 300 rpm for 24 hours at 30° C. to obtain a graphite sol; Then the graphite sol is placed in a liquid phase ball mill and shaped in a sol state to obtain a spherical graphite colloid; Then, the spherical graphite colloid is placed in a mold, and cured and cross-linked for 60 minutes at high temperature and high pressure (60°C, 40MPa pressure) to obtain a gel; Then, the gel solution was centrifuged (8000 rpm) to separate the solid product, which was washed with 50 wt % ethanol aqueous solution until the pH value was 7, and dried at 100 ° C for 5 h to obtain gel-filled natural graphite spheres; The gel-filled natural graphite spheres were carbonized at high temperature (1200°C for 14 h) under N2 protection to obtain modified natural graphite microspheres, which were then demagnetized and sieved to obtain the negative electrode product.
[0038] Comparative Example 4 Method for preparing negative electrode material The natural flake micro powder graphite (200MESH) purchased from Qingdao Langrui Graphite Co., Ltd. was passed through a 200 mesh sieve to obtain the undersize; Then, the above-mentioned undersize (4KG) was added into a 40wt% hydrogen fluoride aqueous solution (10KG) and rapidly stirred (180rpm, 30min), and then filtered to obtain the primary purified modified graphite; Then, the above-mentioned primary purified modified graphite (4KG) was added into a 20% ethanol aqueous solution of hydrogen fluoride (4KG) and stirred continuously (stirring speed 600rpm, 30min) to obtain a suspension; wherein the weight ratio of ethanol to water was 1:4.
[0039] Add resorcinol (0.8 kg) to the graphite suspension, and then continue to stir at high speed for 30 minutes at a stirring speed of 300 rpm to obtain a resorcinol graphite suspension; Add 44 wt % formaldehyde aqueous solution (1.98 kg) in small amounts and repeatedly to the above-obtained resorcinol graphite suspension and continue stirring (300 rpm); after the formaldehyde is completely added, continue stirring at 300 rpm for 24 hours at 30° C. to obtain a graphite sol; Then the graphite sol is placed in a liquid phase ball mill and shaped in a sol state to obtain a spherical graphite colloid; Then, the spherical graphite colloid is placed in a mold, and cured and cross-linked for 60 minutes under high temperature and high pressure (120° C., 250 MPa pressure) to obtain a gel; Then, the gel solution was centrifuged (8000 rpm) to separate the solid product, which was washed with 50 wt % ethanol aqueous solution until the pH value was 7, and dried at 100 ° C for 5 h to obtain gel-filled natural graphite spheres; The gel-filled natural graphite spheres were carbonized at high temperature (900°C for 14 h) under N2 protection to obtain modified natural graphite microspheres, which were then demagnetized and sieved to obtain the negative electrode product.
[0040] Experimental Example 1 The materials obtained in the above embodiments and comparative embodiments are used as negative electrodes, respectively mixed with an aqueous binder (styrene-butadiene rubber SBR) and a conductive agent (carbon black SP) in a mass ratio of 90:7:3, applied to a copper foil, and then dried at 90°C to 110°C, and rolled and dried to form an original sheet as a negative electrode sheet, wherein the coating density of the negative electrode material and the mixture of the aqueous binder and the conductive agent is 10 mg / cm2, and the compaction density is 1.3 g / cm3; a metal lithium sheet is selected as a counter electrode, a diaphragm is a PE material with a thickness of 13 μm, a porosity of about 48%, an electrolyte is ethylene carbonate (EC) + propylene carbonate (PC) = 1:1, 5% of the total mass of fluoroacetate (FEC) and 1.0 mol·L-1 LIF6 are added, a button cell model CR2032 is assembled, and a lithium ion battery is obtained, and the gram capacity, first coulomb efficiency, cell rate and cycle performance of the negative electrode material are detected; The full charge expansion rate of the electrode = (100% SOC electrode thickness - rolling thickness) / (rolling thickness - copper foil thickness) * 100% Among them, the detection methods of gram capacity and first coulomb efficiency are as follows: Standstill → 0.6mA constant current discharge to 5mv → Standstill → 0.2mA constant current discharge to 5mv → Standstill → 0.05mA constant current discharge to 5mv → Standstill → 0.6mA constant current charge to 2V.
[0041] Record the discharge capacity and charge capacity of this process, calculate the mass of the active material on the electrode, and thus calculate its charge-discharge specific capacity in mAh / g. The charge capacity divided by the discharge capacity gives the first charge-discharge efficiency. m active material = (m pole piece - m copper foil) × active material % Discharge capacity in grams = C discharge / m active material Charge capacity in grams = Ccharge / m active material First discharge efficiency = charging gram capacity / discharging gram capacity × 100%; The detection method of battery fast charging is as follows: Standstill → 0.1C constant current discharge to 5mv → Standstill → 0.05C constant current discharge to 5mv → Standstill → 0.1C constant current charge to 2v → Standstill → 0.1C constant current discharge to 5mv → Standstill → 4C constant current charge to 2v; Record the discharge capacity and charge capacity of this process; 4C retention rate = 4C constant current charging capacity / 0.1C constant current charging capacity * 100%.
[0042] The test method of cycle performance is as follows: Standstill → 0.1C constant current discharge to 5mv → Standstill → 0.05C constant current discharge to 5mv → Standstill → 0.5C constant current charge to 2v → Standstill → 0.5C constant current discharge to 5mv → Repeat 0.5C constant current charge & 0.5C constant current discharge; Record the discharge capacity and charge capacity of this process; 500-week cycle retention rate = 0.5C constant current charging capacity in the 500th week / 0.5C constant current charging capacity in the 1st week.
[0043] Table 1 below lists various parameters of the batteries of various examples and comparative examples tested in Experimental Example 1.
[0044] Table 1
[0045] It can be seen from the results of the above embodiments and comparative embodiments that the expansion rate of the negative electrode material prepared using the method of the present invention is greatly reduced, the rate is maintained at the highest, and the reversible capacity, first efficiency and cycle retention rate of the material also maintain the best performance under the process conditions of the present invention.
[0046] It can be seen from the results of Comparative Example 2 that when the mass ratio of resorcinol to graphite is too low (0.04:1), the first efficiency, capacity, rate and cycle performance of the material are worse than those of the embodiment.
[0047] It can be seen from the results of Comparative Example 3 that when the curing and cross-linking temperature and pressure are too low (60°C / 40MPa), the first efficiency, capacity, rate and cycle performance of the material are worse than those of the embodiment.
[0048] It can be seen from the results of Comparative Example 4 that when the carbonization temperature is lower than 1000°C (900°C), the expansion rate of the material is large, and the first efficiency, capacity, rate and cycle performance are worse than those of the embodiment.
[0049] The results of Example 1 and Comparative Example 1 show that the natural graphite modified negative electrode material prepared by the method of the present invention can significantly reduce the expansion rate of the material, and improve the initial efficiency, capacity, cycle and rate performance of the material compared to conventional natural graphite.
[0050] From the test data of the negative electrode material prepared by the embodiment of the present invention and applied in the battery, it can be seen that the material prepared by the preparation method of the present invention has excellent electrochemical properties. Applying it in the battery can significantly improve the first coulombic efficiency and reversible capacity of the battery, and improve the rate and cycle performance of the battery cell.
Claims
1. A method for preparing a negative electrode material, The following steps are involved: S1. Sieving and classifying natural flake graphite powder to obtain raw materials; S2, adding the above raw materials to an aqueous solution of hydrogen fluoride and stirring, then filtering and washing to obtain a primary purified modified graphite; then adding the above primary purified modified graphite to an ethanol aqueous solution of hydrogen fluoride and continuing to stir to obtain a suspension; S3, adding resorcinol and formaldehyde to the suspension under stirring, and continuing stirring to obtain a graphite sol; S4, placing the graphite sol in a liquid phase spheroidizing shaping machine, shaping it in a sol state to obtain a spherical graphite colloid; S5, curing and cross-linking the spherical graphite colloid under high temperature and high pressure to obtain a gel; S6, centrifugally separating the above gel to obtain a solid product, washing it with a mixture of water and ethanol until it is neutral, and drying it to obtain a gel-filled natural graphite sphere; S7. Carbonizing the above-mentioned gel-filled natural graphite spheres under the protection of an inert atmosphere to obtain modified natural graphite microspheres, and obtaining negative electrode materials after demagnetization and screening.
2. The preparation method according to claim 1, wherein In step S1, the flake graphite is flaky crystalline graphite, and the carbon content of the flake graphite is above 95%; The natural flake micro-powder graphite is passed through a 50-450 mesh sieve, and the sieve residue is taken to obtain a raw material.
3. The preparation method according to claim 1, wherein In step S2, the concentration of the hydrogen fluoride aqueous solution is 20-60 wt%, preferably 30-50 wt%, more preferably 40 wt%, the mass ratio of the raw material to the hydrogen fluoride aqueous solution is 1:(0.5-10), preferably 1:(1-5); the stirring speed is 30 rpm-1000 rpm; the stirring time is 20-60 min; The mass ratio of the primary purified modified graphite to the ethanol aqueous solution of hydrogen fluoride is 1: (0.2-5); preferably 1: (0.5-2); the stirring speed is 30rpm-1000rpm; the stirring time is 20-60 min; in the ethanol aqueous solution of hydrogen fluoride, the concentration of hydrogen fluoride is 20-60 wt%, preferably 30-50 wt%, and a mixture of ethanol and water is used as a solvent, and the weight ratio of ethanol to water is 1: (3-5).
4. The preparation method according to claim 1, wherein In step S3, resorcinol is added to the graphite suspension and stirred to obtain a resorcinol graphite suspension. in, The mass ratio of graphite to resorcinol is 1:(0.05-0.5), the stirring time is 15-60min, and the stirring speed is 30rpm-1000rpm; Add formaldehyde to the above-obtained resorcinol graphite suspension and stir, wherein the molar ratio of resorcinol to formaldehyde is 1:(1-4); after the formaldehyde is completely added, stir continuously at 30-45° C. and 30 rpm-1000 rpm for 16-48 hours to obtain a graphite sol.
5. The preparation method according to claim 1, wherein In step S5, curing is performed at a temperature of 70-200° C. and a pressure of 50-400 MPa for 10-120 min to obtain a gel.
6. The preparation method according to claim 1, wherein In step S6, centrifugal separation is performed at 6000-12000 rpm, washed with 30-70 wt % ethanol aqueous solution, and dried at a temperature of 80-120° C. for 3-7 hours.
7. The preparation method according to claim 1, wherein In step S7, the inert atmosphere is nitrogen, the high temperature carbonization temperature is 1000-1300°C, and the carbonization time is 2-24h.
8. A negative electrode material prepared according to the preparation method according to any one of claims 1 to 7.
9. A lithium ion battery comprising the negative electrode material according to claim 8.
Citation Information
Patent Citations
Method for coating artificial graphitic carbon anode material surface
CN103072974A
Application by using carbon nanotube / urea formaldehyde resin carbon-coated spherical microcrystalline graphite as negative electrode material of lithium ion battery
CN107959028A
High-tap-density graphite negative electrode material and preparation method thereof
CN111370694A
Graphite particle, carbon-graphite composite particle and their production processes
WO2007069664A1