Preparation method of porous carbon material for improving first coulombic efficiency

By forming a phosphorene network in phenolic resin-based porous carbon and building a fluorine-rich interface SEI layer, the conductivity and interface stability of porous carbon materials are solved, and the capacity and Coulomb efficiency of lithium-ion batteries are improved, which is suitable for batteries and super capacitors and other fields.

CN118908208AActive Publication Date: 2024-11-08ZHEJIANG GEYUAN NEW MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410768803.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-11-08
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

The existing porous carbon materials have problems such as low electronic conductivity, slow ion diffusion rate, and unstable interface SEI in lithium-ion batteries, which affect their cycling stability and capacity performance.

Method used

By introducing two-dimensional phosphorene materials into the porous carbon of phenolic resin, a phosphorene network is formed using spray granulation technology, and a fluorine-rich interface SEI layer is constructed in combination with fluorocarbon resin to improve the conductivity and interface stability of the silicon carbon negative electrode.

Benefits of technology

The capacity of silicon carbon negative electrode and the first Coulomb efficiency are significantly improved, the specific surface area and conductivity of porous carbon materials are improved, and its performance stability in batteries and supercapacitors is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908208A_ABST
    Figure CN118908208A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a porous carbon material for improving first coulombic efficiency, which comprises the following steps: uniformly mixing a phenolic resin-based carbon precursor, a phosphorene dispersion solution and an organic solvent to obtain a suspension of a phenolic resin composite material containing phosphorus and phosphorene, mixing the suspension with a fluorocarbon resin solution, and carrying out spray granulation to obtain the porous carbon material for improving the first coulombic efficiency. Carrying out ball milling and high-temperature carbonization on the obtained particles to obtain secondary carbon particles containing a fluorocarbon layer; and sequentially carrying out alkali activation and water vapor activation to obtain the surface fluorine-rich type three-dimensional phosphorene riveted porous carbon material. A two-dimensional phosphorene material is introduced into phenolic resin-based porous carbon, and three-dimensional riveting of a phosphorene network in the phenolic resin-based porous carbon material is realized through spray granulation, so that the electrochemical performance of the novel silicon-carbon negative electrode is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous carbon material preparation, and in particular relates to a method for preparing a porous carbon material with improved first coulombic efficiency. Background Art

[0002] Compared with graphite anode (specific capacity 372mAh / g), the theoretical specific capacity of silicon-based anode can reach 4200mAh / g, and its lithium potential (about 0.4V) is similar to that of graphite anode (about 0.1V), so silicon-based anode is considered to be the first choice for the next generation of anode materials. However, there are also some problems with silicon-based anode in actual use, such as severe volume expansion effect (300%) during lithium ion deintercalation, low electron and ion conductance of silicon-based anode, and unstable SEI film during electrochemical charge and discharge, which have negative effects on the cycle stability of silicon-based anode. In order to solve these problems, the use of carbon materials to coat and modify silicon anode is considered to be the ultimate solution. Recently, the use of nano-silicon vapor deposition into porous carbon materials to obtain new silicon-carbon anode materials has attracted much attention in the industry. However, there is still a lot of room for development in the regulation of the physicochemical properties of porous carbon (such as specific surface area, pore volume, pore size distribution, and electron ion conductivity). As an important raw material for preparing porous carbon skeletons, phenolic resin is widely used in the preparation of porous carbon materials. However, the porous carbon negative electrode prepared by phenolic resin has many problems such as low electronic conductivity, slow ion diffusion rate, unstable interface SEI, etc. The existing solution is mainly to modify the conductivity of phenolic resin by N and P doping. However, this doping modification cannot form a three-dimensional continuous conductive network, has limited improvement on the overall conductivity of its conductivity, and cannot build a relatively stable electrode-electrolyte interface SEI film. The existing silicon-carbon negative electrode materials still have low electronic conductivity, poor lithium ion diffusion capacity, and unstable interface. The modification of phenolic resin-based carbon skeleton is of great significance for the regulation of the physical and chemical properties of new silicon-carbon negative electrode materials.

[0003] CN117691059A discloses a composite black phosphorus-based phosphorus-carbon negative electrode material and a preparation method thereof. The specific preparation steps are as follows: (1) preparing a mesoporous carbon material dispersion: ultrasonically mixing the mesoporous carbon material and a solvent in a certain proportion, stirring and mixing for a certain period of time to finally obtain a mesoporous carbon material dispersion; (2) preparing a black phosphorus dispersion: dispersing the powder obtained by ball milling black phosphorus in a solvent while stirring, and finally obtaining a uniformly mixed black phosphorus dispersion; (3) preparing a composite black phosphorus-based phosphorus-carbon negative electrode material: slowly dripping the above black phosphorus dispersion into the mesoporous carbon material dispersion, followed by ultrasonic oscillation and solvent / hydrothermal reaction, and collecting and vacuum freeze-drying the product after centrifugal washing for multiple times, and placing the freeze-dried final product in an agate mortar for crushing and grinding to obtain the desired composite black phosphorus-based phosphorus-carbon negative electrode material. CN112018363A discloses a composite black phosphorus-based phosphorus-carbon negative electrode material and a preparation method thereof, wherein the carbon material and the black phosphorus are covalently bonded to the black phosphorus through high-energy ball milling treatment, thereby forming a black phosphorus-carbon modified composite material, and the conductive polymer is continuously or discontinuously coated on the surface of the black phosphorus-carbon modified composite material through liquid phase in-situ polymerization, thereby obtaining the desired black phosphorus-based composite negative electrode material, and wherein, based on the total weight of the black phosphorus-based composite negative electrode material, the coating amount of the conductive polymer is 0.01-50wt%; the conditions of the high-energy ball milling treatment are: the feed mass ratio of black phosphorus and carbon material is 0.05-20:1; the ball-to-material mass ratio is 10-300:1; the ball milling speed is 300-1000rpm; and the ball milling time is 1-12h.

[0004] In the above-mentioned mixed method, the black phosphorus material is filled into the mesopores of the carbon material. The black phosphorus material occupies a certain void space, which reduces the space for CVD vapor deposition of silicon, thereby reducing the amount of deposited silicon, resulting in a decrease in the capacity of the negative electrode material. At the same time, when black phosphorus is added to the mesopores, the black phosphorus in each void is in a discrete state and cannot form a continuous network, resulting in the added black phosphorus being unable to fully exert its chemical properties. Summary of the invention

[0005] Compared with the existing technology, this technical solution mainly solves: 1) how to improve the electronic and ionic conductivity of phenolic resin-based porous carbon substrates; 2) how to fix phosphorene in phenolic resin-based porous carbon substrates to promote the improvement of conductivity after silicon deposition; 3) how to construct a fluorine-rich interface SEI layer through fluorocarbon resin to stabilize the interface stability between the silicon-carbon negative electrode and the electrolyte.

[0006] In order to achieve the above purpose, this technical solution mainly adopts the following technical means:

[0007] A method for preparing a porous carbon material for improving first coulombic efficiency comprises the following steps:

[0008] (S1) pre-carbonizing a phenolic resin at a high temperature to obtain a phenolic resin-based carbon precursor;

[0009] (S2) adding anionic surfactant to deoxygenated water to prepare a solution, adding black phosphorus crystals, peeling the black phosphorus crystals with a probe ultrasonic instrument, peeling phosphorene from the black phosphorus crystals, separating the unpeeled black phosphorus crystals at the bottom by low-speed centrifugation, and obtaining a phosphorene dispersion solution by liquid phase high-speed centrifugation;

[0010] (S3) uniformly mixing the phenolic resin-based carbon precursor, the phosphorene dispersion solution and the organic solvent to obtain a suspension of the phosphorene-containing phenolic resin composite material;

[0011] (S4) mixing the suspension and the fluorocarbon resin solution, spraying the mixture to form granules, ball milling the obtained particles, and carbonizing them at high temperature to obtain secondary carbon particles containing a fluorocarbon layer;

[0012] (S5) activating the secondary carbon particles of the fluorine-containing carbon layer for the first time in the presence of an alkaline activator to obtain a first activated carbon material;

[0013] (S6) The first activated carbon material is activated for a second time in the presence of water vapor as an activating agent to obtain a second activated carbon material; the second activated carbon material is subjected to acid washing, washing, and drying to obtain a porous carbon material.

[0014] Furthermore, in step (S1), the molecular weight of the phenolic resin is 5000-20000, and the high temperature pre-carbonization is carried out at 500-800°C for 2-3h.

[0015] Furthermore, in step (S2), the anionic surfactant is selected from at least one of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate; the content of the anionic surfactant is 2-5wt%; and the mass ratio of black phosphorus crystals to the anionic surfactant solution is 10-18:100.

[0016] Furthermore, in step (S2), the working parameters of the probe ultrasonic instrument are 20-50kHz, the ultrasonic time is 1-2h, the low-speed centrifugation is centrifugation at a speed of 500-5000rpm for 5-10min, and the high-speed centrifugation is centrifugation at a speed of 10000-30000rpm for 10-30min; the solid content of the obtained phosphorene dispersion solution is 5-10wt%.

[0017] Furthermore, in step (S3), the mass ratio of the phenolic resin-based carbon precursor, the phosphorene dispersion solution and the organic solvent is 100:20-30:150-200.

[0018] Furthermore, in step (S3), the organic solvent is selected from at least one of ethanol, NMP, DMF, and DMSO.

[0019] Furthermore, in step (S4), the fluorocarbon resin is selected from at least one of polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), and polyvinyl fluoride (PVF); the solvent of the fluorocarbon resin solution is N-methylpyrrolidone (NMP), and the concentration of the fluorocarbon resin solution is 10-30wt%; the mass ratio of the suspension to the fluorocarbon resin solution is 100:2.5-5.

[0020] Furthermore, in step (S4), the process parameters of spray granulation are that the pressure is controlled at 0.08-0.1MPa, the feed rate is controlled at 100-300mL / min, and the spray granulation process conditions are controlled so that the D50 of the obtained secondary carbon sphere particles is 5-10μm; high temperature curing is treated at 700-1000℃ for 2-5h under a carbonization inert atmosphere; preferably, the inert atmosphere is at least one of nitrogen, argon, and helium.

[0021] Furthermore, in step (S5), the alkaline activator is potassium hydroxide and / or sodium hydroxide, and the amount of the alkaline activator is 100-300% of the mass of the secondary carbon particles of the fluorine-containing carbon layer; the first activation is treated at 700-800°C for 2-4h.

[0022] Furthermore, in step (S6), the ratio of the water vapor flow rate to the mass of the first activated carbon material is 0.01-0.1 L / min / g, preferably 0.03-0.045 L / min / g.

[0023] Furthermore, in step (S5) and step (S6), the first activation and the second activation are carried out under a protective atmosphere, and the protective atmosphere is at least one of nitrogen, argon and helium.

[0024] Furthermore, in step (S6), the pickling is performed by pickling with 1-10% HCl solution, and the purpose of pickling is to remove the KOH component and part of the ash involved in the alkali activation; the washing is performed by water washing until the filtrate is neutral (pH=7±0.5); and the drying is performed by centrifugal drying, oven drying, vacuum drying, etc.

[0025] The present invention has achieved the following technical effects:

[0026] 1. The present invention introduces two-dimensional phosphorene material into phenolic resin-based porous carbon, and realizes three-dimensional riveting of phosphorene network in phenolic resin-based porous carbon material through spray granulation, thereby improving the capacity and first coulombic efficiency of silicon-carbon negative electrode.

[0027] Second, the present invention realizes the uniform coating of fluorocarbon resin on the surface of porous carbon materials, thereby improving the performance of the product. In addition, by adjusting the molecular weight and type of phenolic resin, as well as the mass ratio of phenolic resin to black phosphorus material, the parameters of carbon material such as pore size, pore volume, and specific surface area can be precisely controlled to meet different application requirements.

[0028] 3. The porous carbon product prepared by the preparation method of the present invention has excellent performance, high specific surface area, good electrical conductivity and chemical stability, and is suitable for use in batteries, supercapacitors, catalyst carriers and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a SEM image of the fluorine-rich three-dimensional phosphorene-riveted porous carbon material prepared in Example 1.

[0030] Figure 2 This is an XRD comparison diagram of the fluorine-rich three-dimensional phosphorene-riveted porous carbon in Example 1 before and after activation and pore formation.

[0031] Figure 3 This is the element mapping diagram of the fluorine-rich three-dimensional phosphorene-riveted porous carbon in Example 1.

[0032] Figure 4 This is a high-resolution XPS image of the F element of the fluorine-rich three-dimensional phosphorene-riveted porous carbon in Example 1.

[0033] Figure 5 This is a high-resolution XPS image of the P element of the fluorine-rich three-dimensional phosphorene-riveted porous carbon in Example 1.

[0034] Figure 6 This is the nitrogen adsorption curve of the fluorine-rich three-dimensional phosphorene-riveted porous carbon in Example 1.

[0035] Figure 7 This is the pore size distribution diagram of the fluorine-rich three-dimensional phosphorene-riveted porous carbon in Example 1.

[0036] Figure 8 This is the powder resistivity curve of the fluorine-rich three-dimensional phosphorene riveted porous carbon pores in Example 1 at 10MPa-100MPa.

[0037] Fig. 9 This is the powder resistivity curve of the porous carbon pores in Comparative Example 1 at 10 MPa-100 MPa. DETAILED DESCRIPTION

[0038] The phenolic resin is prepared by using formaldehyde and phenol in a molar ratio of 1.3:1.

[0039] Example 1

[0040] (S1) selecting a phenolic resin with a molecular weight of 5000 for high-temperature pre-carbonization at a temperature of 500° C. for 2 hours to obtain a phenolic resin-based carbon precursor for standby use;

[0041] (S2) sodium dodecyl sulfate (SDS) is added to deoxygenated water to prepare a 2.5 wt% surfactant solution, black phosphorus crystals are added, the mass ratio of black phosphorus crystals to surfactant solution is 15:100, and the black phosphorus crystals are peeled off by a probe ultrasonic instrument (ultrasonic frequency 20 kHz, ultrasonic time 1-2 h), first centrifuged at 3000 rpm for 5 min to separate the unpeeled black phosphorus crystals at the bottom, and then centrifuged at 10000 rpm for 20 min to obtain a phosphorene dispersion solution;

[0042] (S3) mixing the phenolic resin-based carbon precursor, the phosphorene dispersion solution and ethanol in a mass ratio of 100:20:150 to obtain a suspension of a phenolic resin composite material containing phosphorene;

[0043] (S4) preparing a polyvinylidene fluoride (PVDF) / NMP solution system with a concentration of 10 wt%, mixing the suspension obtained in step (S3) and the PVDF / NMP solution system at a mass ratio of 100:5, spray granulating the mixture (0.08 MPa, feed rate 100 mL / min), and then ball milling to make the D50 of the secondary carbon sphere particles 5-10 μm; then high-temperature carbonization is performed in a tubular furnace (argon protection) at a carbonization temperature of 800° C. for 2 hours to obtain secondary carbon particles uniformly coated with a fluorine-containing carbon layer;

[0044] (S5) uniformly mixing the secondary carbon sphere particles and potassium hydroxide in a mass ratio of 1:1, and performing high-temperature activation (nitrogen protection) at an activation temperature of 800° C. for 2 hours to obtain a first activated carbon material;

[0045] (S6) placing the first activated carbon material in a tubular furnace (under argon protection), and performing secondary activation and pore formation with water vapor, the flow rate of the water vapor is 0.045 L / min / g, the activation temperature is 900° C., and the time is 3 hours. Finally, after acidification, washing, centrifugal drying, a fluorine-rich three-dimensional phosphorene-riveted porous carbon material is finally obtained.

[0046] Figure 1 This is the SEM image of the fluorine-rich three-dimensional phosphorene-riveted porous carbon material prepared in Example 1. It can be seen that it is spherical and quasi-spherical. The phenolic resin carbon precursor, black phosphorus, and fluorocarbon resin form relatively uniform spheres, and then undergo a condensation reaction to form spherical carbon during a high-temperature carbonization process.

[0047] Figure 2This is the XRD comparison diagram of the fluorine-rich three-dimensional phosphorene riveted porous carbon in Example 1 before and after activation and pore formation. It can be seen that the reactants before activation are mainly carbides, and due to the small addition of P and F elements, they are not obvious in XRD. With the high-temperature activation reaction, the C peak in XRD gradually becomes obvious. This is because during the high-temperature activation process, the resin material that was originally not completely carbonized is completely carbonized and presents a stable carbon structure.

[0048] Figure 3 This is the element mapping diagram of the fluorine-rich three-dimensional phosphorene-riveted porous carbon in Example 1, which reflects the doping of P and N elements in the carbon material, and it can be seen that the P and N elements are evenly distributed.

[0049] Figure 4 This is a high-resolution XPS image of the F element of the fluorine-rich three-dimensional phosphorene-riveted porous carbon in Example 1.

[0050] Figure 5 This is a high-resolution XPS image of the P element of the fluorine-rich three-dimensional phosphorene-riveted porous carbon in Example 1. Figure 4 , Figure 5 It can be used to detect the content of F and P in porous carbon materials. At the same time, as shown in Tables 2 and 3, with the increase of the mass ratio of raw material black phosphorus, the content of phosphorus in the carbon material shows a linear trend. When the mass ratio of the raw material is lower than 10%, it shows a conversion rate of about 75%. When it is higher than 10%, the conversion rate of black phosphorus to P in the carbon material is less than 50%. This is because with the excessive increase of the amount of black phosphorus added, the P element is supersaturated in the carbon material, and part of the black phosphorus does not participate in the construction of the three-dimensional network structure of phosphorene. The addition of the F element shows a stable linear trend. With the addition of the F element, it helps to form a stable SEI film. From the analysis of the specific surface, pore volume and pore size, with the increase of P content, the specific surface of porous carbon shows a downward trend. This is because black phosphorus is a very stable structure. The high-temperature activation process will not etch the phosphorene structure, but only activate and etch the internal resin-based carbon material. Phosphorene acts as a phenolic resin carbon connecting matrix in the porous carbon structure, presenting a stable state. At the same time, the phosphorus content increases, and the phosphorene that acts as a rivet between carbon materials increases, increasing the distance between carbons, which significantly increases the pore volume. The addition of F element will not have a significant effect on the pore volume and pore size.

[0051] Figure 6 This is the nitrogen adsorption curve of the fluorine-rich three-dimensional phosphorene-riveted porous carbon in Example 1.

[0052] Figure 7 This is the pore size distribution diagram of the fluorine-rich three-dimensional phosphorene-riveted porous carbon in Example 1.

[0053] Figure 8 This is the powder resistivity curve of the fluorine-rich three-dimensional phosphorene riveted porous carbon pores in Example 1 at 10MPa-100MPa.

[0054] Fig. 9 This is the powder resistivity curve of the porous carbon pores in Comparative Example 1 at 10 MPa-100 MPa.

[0055] Embodiment 2-9

[0056] Examples 1-10 are the same as Example 1, except that the mass ratio of black phosphorus crystals and surfactant solution in step (S2) is different (Examples 2-4), and the concentration of fluorocarbon resin solution in step (S4) is different (Examples 5-10); Examples 11-13 are the same as Example 10, except that Example 11 only performs KOH activation, and Example 12 only performs water vapor activation; Example 13 has a first activation of water vapor activation and a second activation of KOH activation; The preparation process parameters of the examples and comparative examples are listed in Table 1 below;

[0057] Table 1 Process parameters

[0058]

[0059] The porous carbon prepared in the above examples and comparative examples was tested for specific surface area, pore size distribution, pore volume, phosphorus content, fluorine content, and resistivity. The results are shown in Table 2.

[0060] Table 2 Porous carbon parameter test

[0061]

[0062] Application Examples

[0063] The porous carbon of the above-mentioned embodiments and comparative examples was prepared into silicon-carbon negative electrode materials, and the battery was assembled to test the first cycle charge and discharge specific capacity and the first effect. Specifically, 1 kg of porous carbon was first placed in a rotary kiln, and Ar was introduced as a protective gas. The rotary kiln speed was 60 r / min, and the temperature was kept stable after rising to 500 ° C. Then, silane gas was introduced at a flow rate of 3 L / min for 4.5 hours, and silane was cracked into Si and deposited in the gaps of the porous carbon. After the silicon-carbon material was formed, the introduction of silane gas was stopped. Then, the temperature was raised to 900 ° C, and acetylene gas was introduced at a flow rate of 3 L / min for 2 hours. Acetylene was cracked into carbon coated on the surface of the deposited silicon-carbon to form an active substance of the negative electrode material of a lithium battery. The obtained silicon-carbon active material was used as the negative electrode of the battery for electrochemical testing. Specifically, the active material, polyacrylic acid (PAA), and superP were mixed in deionized water in a mass ratio of 8: 1: 1, and after being fully ground, they were placed in a homogenizer to prepare a slurry. Then, the slurry was evenly coated on the copper foil with a thickness of 200um and placed in a vacuum drying oven for drying. Subsequently, a 12mm pole piece was made by a punching machine and placed in a vacuum glove box. A 16mm lithium sheet was selected as a symmetrical electrode, Celgard2600 was selected and cut into 18mm pieces as a diaphragm, and a 1M LiPF6 electrolyte (the solvent was 1:1:1 in the volume ratio of EC:EDC:EMC, and 5% FEC was added) was selected to prepare a CR2032 button cell. The blue electric system was selected for electrochemical testing. Specifically, the battery was left to stand for 1 hour, then discharged at a rate of 0.1C until the voltage dropped to 0.005V, then left to stand for 1 hour, then discharged at a rate of 0.02C until the voltage dropped to 0.005V, then left to stand for 1 hour, then discharged at a rate of 0.01C until the voltage dropped to 0.005V, and then charged at a rate of 0.1C until the voltage reached 1.5V and then stopped. The results are shown in Table 3.

[0064] Table 3 Electrochemical performance test

[0065]

Claims

1. A method for preparing a porous carbon material with improved first coulombic efficiency, characterized in that: The following steps are involved: (S1) pre-carbonizing a phenolic resin at a high temperature to obtain a phenolic resin-based carbon precursor; (S2) adding anionic surfactant to deoxygenated water to prepare a solution, adding black phosphorus crystals, peeling the black phosphorus crystals with a probe ultrasonic instrument, peeling phosphorene from the black phosphorus crystals, separating the unpeeled black phosphorus crystals at the bottom by low-speed centrifugation, and obtaining a phosphorene dispersion solution by liquid phase high-speed centrifugation; (S3) uniformly mixing the phenolic resin-based carbon precursor, the phosphorene dispersion solution and the organic solvent to obtain a suspension of the phosphorene-containing phenolic resin composite material; (S4) mixing the suspension and the fluorocarbon resin solution, spraying the mixture to form granules, ball milling the obtained particles, and carbonizing them at high temperature to obtain secondary carbon particles containing a fluorocarbon layer; (S5) activating the secondary carbon particles of the fluorine-containing carbon layer for the first time in the presence of an alkaline activator to obtain a first activated carbon material; (S6) activating the first activated carbon material for a second time in the presence of water vapor as an activating agent to obtain a second activated carbon material; The second activated carbon material is subjected to acid washing, washing and drying to obtain a porous carbon material.

2. The preparation method according to claim 1, characterized in that: In step (S1), the molecular weight of the phenolic resin is 5000-20000, and the high temperature pre-carbonization is 500-800°C for 2-3h.

3. The preparation method according to claim 1, characterized in that: In step (S2), the anionic surfactant is selected from at least one of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate; the content of the anionic surfactant is 2-5wt%; and the mass ratio of black phosphorus crystals to the anionic surfactant solution is 10-18:

100.

4. The preparation method according to claim 1, characterized in that: In step (S2), the working parameters of the probe ultrasonic instrument are 20-50kHz, the ultrasonic time is 1-2h, the low-speed centrifugation is centrifugation at a speed of 500-5000rpm for 5-10min, and the high-speed centrifugation is centrifugation at a speed of 10000-30000rpm for 10-30min; the solid content of the obtained phosphorene dispersion solution is 5-10wt%.

5. The preparation method according to claim 1, characterized in that: In step (S3), the mass ratio of the phenolic resin-based carbon precursor, the phosphorene dispersion solution and the organic solvent is 100:20-30:150-200.

6. The preparation method according to claim 1, characterized in that: In step (S4), the fluorocarbon resin is selected from at least one of polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), and polyvinyl fluoride (PVF); the solvent of the fluorocarbon resin solution is N-methylpyrrolidone (NMP), and the concentration of the fluorocarbon resin solution is 10-30wt%; the mass ratio of the suspension to the fluorocarbon resin solution is 100:2.5-5.

7. The preparation method according to claim 1, characterized in that: In step (S4), the process parameters of the spray granulation are that the pressure is controlled at 0.08-0.1 MPa, the feed rate is controlled at 100-300 mL / min, and the spray granulation process conditions are controlled so that the D50 of the obtained secondary carbon sphere particles is 5-10 μm; High temperature curing is a treatment at 700-1000° C. for 2-5 hours in a carbonization inert atmosphere; preferably, the inert atmosphere is at least one of nitrogen, argon and helium.

8. The preparation method according to claim 1, characterized in that: In step (S5), the alkaline activator is potassium hydroxide and / or sodium hydroxide, and the amount of the alkaline activator is 100-300% of the mass of the secondary carbon particles of the fluorine-containing carbon layer; the first activation is treated at 700-800°C for 2-4h.

9. The preparation method according to claim 1, characterized in that: In step (S6), the ratio of the water vapor flow rate to the mass of the first activated carbon material is 0.01-0.1 L / min / g, preferably 0.03-0.045 L / min / g.

10. The preparation method according to claim 1, characterized in that: In step (S6), the acid washing is performed by using a 1-10% HCl solution; the washing is performed by washing with water until the filtrate is neutral; and the drying is performed by centrifugal drying, oven drying or vacuum drying.

Citation Information

Patent Citations

  • Preparation method of phosphorus-doped porous carbon negative electrode material with improved first coulomb efficiency

    CN107623118A

  • Phosphorus quantum dot composited porous hard carbon material, as well as preparation method and application thereof

    CN109301194A

  • Carbon nitride membrane composite material modified by black phosphorus / metal organic framework, and preparation method thereof and application in waste gas treatment

    US20190381487A1