High-purity, high-hardness and high-density oxygen-free boron block and preparation method thereof

By adding boron carbide additives to the boron powder to remove oxygen impurities and using advanced sintering technology, the preparation problem of high-purity oxygen-free boron blocks is solved, and the preparation of boron blocks with high hardness, high density and low cost is achieved.

CN118908235AActive Publication Date: 2024-11-08WUHAN UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411126871.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-08
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

It is difficult to obtain high purity, high hardness and high density oxygen-free boron blocks in the prior art, and the sintering window of boron is narrow and easy to crack, making the preparation process complex and costly.

Method used

By adding boron carbide or boron and carbon mixture to boron powder as additives, chemical reactions are used to remove oxygen impurities to form high-purity oxygen-free boron blocks, and using pressure-free sintering, hot press sintering or discharge plasma sintering technology, it is optimized Sintering parameters for densification and performance improvement.

Benefits of technology

The preparation of oxygen-free boron blocks with high purity, high hardness and high density is achieved, which simplifies the process flow, reduces manufacturing costs, and improves the mechanical properties and economic benefits of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908235A_ABST
    Figure CN118908235A_ABST
Patent Text Reader

Abstract

The invention relates to the field of non-oxide structural ceramics, in particular to a high-purity, high-hardness and high-density oxygen-free boron block and a preparation method thereof.The preparation method comprises the steps that commercially available boron powder and boron carbide powder or a mixture of boron and carbon serve as raw materials, the powder is proportioned, and the raw material powder is mixed, dried and sieved to obtain the high-purity, high-hardness and high-density oxygen-free boron block. And sintering in a pressureless sintering, hot pressed sintering or discharge plasma sintering environment to obtain the required oxygen-free boron block. According to the method, B6O can be removed by changing the content of the additive added into the boron powder, then the oxygen-free boron block with high purity, high hardness and high density is obtained, and the microstructure and the mechanical property of the oxygen-free boron block are regulated in situ.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of non-oxide structural ceramics, and in particular to a high-purity, high-hardness and high-density oxygen-free boron block and a preparation method thereof. Background Art

[0002] Boron (B) is widely used in various fields such as cutting tools, thermoelectric energy conversion materials, semiconductor targets, thrusters and nuclear energy applications because of its light weight, high strength, high hardness and high melting point. At the same time, elemental boron is an efficient neutron absorber (~3840 barns) in the atomic energy industry. There are two main types of boron powder on the market. One is a micron-sized amorphous boron powder obtained by metal reduction method using boron oxide and magnesium reducing agent as raw materials. When boron is produced by this method, the purity of crude boron is 80%, which is more than 95% after purification, but the oxygen content is relatively high. The other type is a crystalline boron powder obtained by regional melting of boron powder to obtain a crystal block of boron, and then crushing it. It has the advantages of high purity and low oxygen content, but the grain size is large and sintering is difficult.

[0003] High-purity boron powder is difficult to obtain and expensive. The melting point of boron is only 2076 ° C, and its sintering window is very narrow, which makes it difficult to sinter and the block is easy to crack. Another type of process for preparing high-purity boron is obtained by reducing haloborane with hydrogen. The reaction between gases not only has a low yield, but also a complex synthesis device and high manufacturing cost. (DRStern; Lynds, Lahmer. High-Purity Crystalline Boron. Journal of the Electrochemical Society. 1958, 105 (11): 676.). Recently, Zhang et al. used commercial boron powder as a raw material to densify polycrystalline rhombic boron blocks by spark plasma sintering (SPS) (Journal of Materials Science & Technology, 2022, 99: 148-160). The hardness and fracture toughness of the prepared β-B are approximately 31GPa and 2.2MPa m1 / 2, respectively. The results show that the in-situ grown nano-boron-rich oxide enhances the densification and mechanical properties of β-B. However, the presence of oxides is not conducive to some applications that require the application of high-purity boron, such as semiconductor pure boron targets. Therefore, with the growing demand for high-precision applications, the preparation of high-purity oxygen-free boron blocks is of great significance.

[0004] For commercial boron powder, some low melting point metal oxides inevitably appear in the starting boron powder. The oxygen remaining in the boron powder is difficult to completely remove by post-treatment, and these oxygen impurities will also make subsequent sintering difficult and prone to cracking.

[0005] In view of this, the present invention can not only achieve sintering densification of boron powder by adding a small amount of additives to the boron powder, but also remove impurities such as B6O in the boron block in situ to obtain a pure, oxygen-free, and excellent mechanical property elemental boron block. Summary of the invention

[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide a high-purity, high-hardness and high-density oxygen-free boron block and a preparation method thereof. The present invention uses commercial boron powder as a starting material, and the oxygen impurities remaining in the powder react with elemental boron in situ to generate submicron-scale boron-rich oxides (e.g., B6O grains), and the oxygen impurities are difficult to completely remove by post-processing means. In this regard, the present invention can not only remove oxygen from the boron block by additionally adding auxiliary agents such as boron carbide or a mixture of boron and carbon, but also form additional boron during the reaction process, which has the advantage of increasing the yield of pure boron. The pure boron block obtained by this method has the characteristics of uniform structure, grain refinement, and excellent mechanical properties.

[0007] To achieve the above object, the present invention is implemented by the following technical solutions:

[0008] The present invention provides a high-purity, high-hardness and high-density oxygen-free boron block, which uses commercially available boron powder and boron carbide powder or a boron-carbon mixture as raw materials, and the raw materials are mixed according to any one of the following chemical reaction equations (1) to (3):

[0009] (100-y) B + y B2O3 + 3y B x C=(100+13y) B + 3y CO (1)

[0010] (100-y) B + y B2O3 + 3y B4C=(100+13y) B + 3y CO (2)

[0011] (100-y) B + y B2O3 + 3y C=(100+y) B + 3y CO (3)

[0012] Among them, the value range of parameter x is: 4≤x≤10.5; the value range of parameter y is: 0≤y≤100. The value of x depends on the solid solubility of boron carbide, that is, the boron-carbon ratio; the value of y depends on the oxygen content in the actual boron powder. The oxygen content in commercially available boron powder varies. According to reaction formula (4), powder with a higher oxygen content will also form a boron block with a higher boron-rich oxide content after sintering. According to chemical reaction formula (5), adding additives such as boron carbide powder or a mixture of boron and carbon to the boron powder will gradually consume the boron-rich oxide that has been formed. Impurities such as Mg that are easily volatilized in the boron are removed through in-situ vacuum treatment during the sintering process, and finally a high-purity boron block without oxide is formed.

[0013] 16 B + B2O3=3 B6O (4)

[0014] B6O+ B4C=10 B + CO (5)

[0015] As a further optimization solution of the present invention, the carbon is graphite or carbon black.

[0016] As a further optimization scheme of the present invention, the purity of the graphite is greater than 99%, and the particle size is 0.5-100 μm; the purity of the carbon black is greater than 99%, and the particle size is 5-500 nm.

[0017] As a further optimization scheme of the present invention, the purity of the B4C is greater than 99%, and the particle size is 0.5-5 μm; when x=6, the purity of the B6C is greater than 99%, and the particle size is 1-5 μm.

[0018] The present invention also provides a method for preparing the high-purity, high-hardness and high-density oxygen-free boron block, the preparation method comprising:

[0019] Step 1, weighing raw material powders according to the proportion of the designed chemical reaction equation, mixing, drying and sieving the raw material powders;

[0020] Step 2: Pour the raw material powder obtained in step 1 into a mold, and sinter it under pressureless sintering, hot pressing sintering or spark plasma sintering to obtain the required oxygen-free boron block. Densification and performance optimization of the boron block can be achieved by changing parameters such as sintering temperature, holding time, loading pressure, and heating rate.

[0021] As a further optimization solution of the present invention, in step 2, the sintering environment is a vacuum or flowing argon atmosphere.

[0022] As a further optimization scheme of the present invention, in the step 2, the sintering temperature ranges from 1600°C to 2000°C.

[0023] As a further optimization scheme of the present invention, in step 2, the insulation time ranges from 5 to 180 minutes.

[0024] As a further optimization scheme of the present invention, in step 2, the loading pressure range is 5-75 MPa.

[0025] As a further optimization scheme of the present invention, in step 2, the heating rate ranges from 10 to 300° C. / min.

[0026] The technical solution provided by the present invention has the following beneficial effects:

[0027] (1) B6O particles are inevitably formed in the boron block sintered from the initial boron powder, and a pure boron block cannot be obtained. The present invention removes B6O by adding boron carbide or a mixture of boron and carbon as an auxiliary agent and changing the content of the auxiliary agent, which can effectively remove oxygen impurities in the boron powder and form additional pure boron during the reaction process, thereby obtaining a high-purity, high-hardness and high-density oxygen-free boron block, and in-situ regulating its microstructure and mechanical properties, which is particularly important for applications requiring high-purity boron (such as semiconductor pure boron targets).

[0028] (2) The additives added in the present invention not only help deoxidation, but also promote densification during the sintering process, so that the final boron block has a higher density. High density means fewer pores and defects, which is crucial for improving the mechanical properties of the material. The present invention utilizes advanced sintering technologies such as pressureless sintering, hot pressing sintering or spark plasma sintering (SPS), combined with reasonable sintering parameters (such as sintering temperature, holding time, loading pressure and heating rate), to achieve densification of the boron block, avoid cracking, and improve the overall performance of the block.

[0029] (3) The chemical reaction equation in the present invention provides a variety of raw material ratios for selection, and the y value can be flexibly adjusted according to the oxygen content in the commercially available boron powder, thereby optimizing the reaction process and product performance. At the same time, the flexible adjustment of sintering parameters also provides more possibilities for performance optimization.

[0030] (4) Compared with the traditional high-purity boron preparation process, the method of the present invention not only simplifies the preparation process and reduces the complexity of the equipment, but also improves the yield and purity, thereby having lower manufacturing costs and higher economic benefits.

[0031] (5) The raw materials of the present invention are easy to obtain, the preparation process is mature, and the cycle is short. The sintering densification of the boron block can be achieved at 1600°C-2000°C, which is beneficial to reducing the energy consumption required in the material preparation process. The obtained boron block has a high density. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The microscopic morphology of the sample was obtained for Comparative Example 2;

[0033] Figure 2 The XRD of the sample was obtained for Comparative Example 2;

[0034] Figure 3 The microscopic morphology of the sample was obtained for Comparative Example 3;

[0035] Figure 4 The XRD of the sample obtained for Comparative Example 3;

[0036] Figure 5 The microscopic morphology of the sample obtained in Example 1;

[0037] Figure 6 The microscopic morphology of the sample obtained in Example 2. DETAILED DESCRIPTION

[0038] In order to enable those skilled in the art to better understand the technical solution of the present invention, the preferred implementation scheme of the present invention is described below in conjunction with specific embodiments, but it should not be understood as limiting the present invention and is only used as an example.

[0039] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.

[0040] Comparative Example 1

[0041] Boron powder (purity of 95%, particle size of 0.1-5 μm) is used as raw material, and the obtained boron sample contains 16% (volume content) of B6O as a second phase.

[0042] The weighed powder is soaked in ethanol (purity>99%) solvent for 1-6 hours, and the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is crushed and sieved, poured into a graphite mold, and pressure sintered using a spark plasma sintering device. The entire process is carried out under vacuum.

[0043] The sintering process includes the following steps: room temperature to 450°C, the heating rate is 100°C / min, and the pressure applied to the sample is 5MPa. Then the pressure is increased to 60MPa within 2min. From 450°C to 2000°C, the heating rate is 100°C / min, and the pressure is 60MPa. After keeping at 2000°C for 5min, the pressure is reduced to 5MPa and heating is stopped, and the sample is cooled to room temperature with the furnace.

[0044] Compared with the sample with added additives, the obtained sample contains 16% (volume content) of B6O as the second phase. The relative density of the boron block is 99.8%, the Vickers hardness is 30-38GPa, the three-point bending strength is 140-300MPa, and the fracture toughness is 2.5-3.5MPam 0.5 , the room temperature thermal conductivity is 15-20W / mK.

[0045] Comparative Example 2

[0046] Boron powder (purity of 95%, particle size of 0.1-5 μm) is used as raw material, and the obtained boron sample contains 16% (volume content) of B6O as a second phase.

[0047] The weighed powder is soaked in ethanol (purity>99%) solvent for 1-6 hours, and the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is crushed and sieved, poured into a graphite mold, and pressure sintered using a spark plasma sintering device. The entire process is carried out under vacuum.

[0048] The sintering process includes the following steps: room temperature to 450°C, the heating rate is 300°C / min, and the pressure applied to the sample is 5MPa. Then the pressure is increased to 60MPa within 2min. From 450°C to 1800°C, the heating rate is 300°C / min, and the pressure is 60MPa. After keeping at 1800°C for 5min, the pressure is reduced to 5MPa and the heating is stopped. The sample is cooled to room temperature with the furnace. The morphology and XRD spectrum of the sintered samples are shown as follows: Figure 1 and Figure 2 shown.

[0049] Compared with the sample with added additives, the obtained sample contains 16% (volume content) of B6O as the second phase. The relative density of the boron block is 99.2%, the Vickers hardness is 30-38GPa, the three-point bending strength is 140-300MPa, and the fracture toughness is 2-3MPa m 0.5 , the room temperature thermal conductivity is 12-18W / mK.

[0050] Figure 1 The microscopic morphology of the sample obtained in Comparative Example 2; it can be seen from the figure that the gray is the boron matrix and the white is the boron-rich oxide grains.

[0051] Figure 2 The XRD of the sample obtained for Comparative Example 2; it can be seen from the figure: two typical phases corresponding to the microscopic morphology.

[0052] Comparative Example 3

[0053] Boron powder (purity of 95%, particle size of 0.1-5 μm) is used as raw material, and the obtained boron sample contains 7% (volume content) of B6O as a second phase.

[0054] The weighed powder is soaked in ethanol (purity>99%) solvent for 1-6 hours, and the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is crushed and sieved, poured into a graphite mold, and pressure sintered using a spark plasma sintering device. The entire process is carried out under vacuum.

[0055] The sintering process includes the following steps: room temperature to 450°C, the heating rate is 50°C / min, and the pressure applied to the sample is 5MPa. Then the pressure is increased to 60MPa within 2min. From 450°C to 1600°C, the heating rate is 50°C / min, and the pressure is 60MPa. After keeping at 1600°C for 5min, the pressure is reduced to 5MPa and the heating is stopped. The sample is cooled to room temperature with the furnace. The morphology and XRD spectrum of the sintered samples are shown as follows: Figure 3 and Figure 4 shown.

[0056] Compared with the addition of additives, the obtained sample contains 16% (volume content) of B6O as the second phase. The relative density of the boron block is 84.8%, the Vickers hardness is 15-25GPa, the three-point bending strength is 140-250MPa, and the fracture toughness is 2.5-3.5MPam 0.5 , the room temperature thermal conductivity is 8-12W / mK.

[0057] Figure 3 The microscopic morphology of the sample obtained in Comparative Example 3; it can be seen from the figure that the gray is the boron matrix, the white is the boron-rich oxide grains, and there are a large number of pores.

[0058] Figure 4 The XRD of the sample obtained for Comparative Example 3 is as follows: two typical phases corresponding to the microscopic morphology.

[0059] Example 1

[0060] Boron powder (purity of 95%, particle size of 0.1-5 μm) and B4C (particle size of 0.5-5 μm) are used as raw materials and the ingredients are prepared according to equation (6):

[0061] 98 B + 2 B2O3+ 6 B4C=126 B + 6 CO (6)

[0062] A pure boron sample without B6O phase was obtained.

[0063] Using ethanol (purity>99%) as solvent and zirconium oxide balls as mixing medium, the weighed powders are mixed and mixed using a mixer at a mixing speed of 30-100rpm. After mixing for 12-36 hours, the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is crushed and sieved and poured into a graphite mold, and pressure sintered using a spark plasma sintering device. The entire process is carried out under vacuum.

[0064] The sintering process includes the following steps: room temperature to 450°C, the heating rate is 300°C / min, and the pressure applied to the sample is 5MPa. Then the pressure is increased to 60MPa within 2min. From 450°C to 1800°C, the heating rate is 300°C / min, and the pressure is 60MPa. After keeping at 1800°C for 5min, the pressure is reduced to 5MPa and the heating is stopped. The sample is cooled to room temperature with the furnace. The morphology of the sintered sample is as follows Figure 5 shown.

[0065] Compared with the sample without additives, the obtained sample is a pure boron sample without B6O phase. The relative density of pure boron block is 98.2%, Vickers hardness is 30-35GPa, three-point bending strength is 140-300MPa, and fracture toughness is 3-3.5MPa m 0.5 , the room temperature thermal conductivity is 20-30W / mK.

[0066] Figure 5 This is the microscopic morphology of the sample obtained in Example 1; it can be seen from the figure that the gray color is the boron matrix and there are no white boron-rich oxide particles.

[0067] Example 2

[0068] Boron powder (purity of 95%, particle size of 0.1-5 μm) and B4C (particle size of 0.5-5 μm) are used as raw materials and the ingredients are prepared according to equation (6):

[0069] 98 B + 2 B2O3+ 6 B4C=126 B + 6 CO (6)

[0070] A pure boron sample without B6O phase was obtained.

[0071] Using ethanol (purity>99%) as solvent and zirconium oxide balls as mixing medium, the weighed powders are mixed and mixed using a mixer at a mixing speed of 30-100rpm. After mixing for 12-36 hours, the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is crushed and sieved and poured into a graphite mold, and pressure sintered using a hot press sintering device. The entire process is carried out under vacuum.

[0072] The sintering process includes the following steps: room temperature to 450°C, the heating rate is 20°C / min, and the pressure applied to the sample is 5MPa. Then the pressure is increased to 60MPa within 2min. From 450°C to 1800°C, the heating rate is 10°C / min, and the pressure is 60MPa. After keeping at 1800°C for 5min, the pressure is reduced to 5MPa and the heating is stopped. The sample is cooled to room temperature with the furnace. The morphology of the sintered sample is as follows Figure 6 shown.

[0073] Compared with the sample without additives, the obtained sample is a pure boron sample without B6O phase. The relative density of pure boron block is 98.2%, Vickers hardness is 30-35GPa, three-point bending strength is 140-300MPa, and fracture toughness is 3-3.5MPa m 0.5 , the room temperature thermal conductivity is 20-30W / mK.

[0074] Figure 6 This is the microscopic morphology of the sample obtained in Example 2; it can be seen from the figure that the gray color is the boron matrix and there are no white boron-rich oxide particles.

[0075] Example 3

[0076] Boron powder (purity of 95%, particle size of 0.1-5 μm) and B4C (particle size of 0.5-5 μm) are used as raw materials and the ingredients are prepared according to equation (6):

[0077] 98 B + 2 B2O3+ 6 B4C=126 B + 6 CO (6)

[0078] The obtained boron sample contained 8% (volume content) of B6O as a second phase.

[0079] Using ethanol (purity>99%) as solvent and zirconium oxide balls as mixing medium, the weighed powders are mixed and mixed using a mixer at a mixing speed of 30-100rpm. After mixing for 12-36 hours, the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is heat-treated using a pressureless sintering device, and the heat-treated powder is crushed and sieved before being pressurelessly sintered again. The entire process is carried out under vacuum.

[0080] The pressureless sintering process includes the following steps: room temperature to 1650℃, heating rate is 10℃ / min, heating is stopped after keeping at 1650℃ for 0.5h, and the sample is cooled to room temperature with the furnace. The pressureless sintering process of the heat-treated powder after crushing and sieving includes the following steps: room temperature to 2000℃, heating rate is 10℃ / min, heating is stopped after keeping at 2000℃ for 3h, and the sample is cooled to room temperature with the furnace.

[0081] Compared with the sample without additives, the obtained sample contains 8% (volume content) of B6O as the second phase. The relative density of the boron block is 91.8%, the Vickers hardness is 20-25GPa, the three-point bending strength is 160-250MPa, and the fracture toughness is 2-2.5MPam 0.5 , the room temperature thermal conductivity is 8-12W / mK.

[0082] Example 4

[0083] Boron powder (purity of 80%, particle size of 0.1-5 μm) and B4C (particle size of 0.5-5 μm) are used as raw materials and the ingredients are prepared according to equation (7):

[0084] 93 B + 7 B2O3+ 21 B4C=191 B + 21 CO (7)

[0085] A pure boron sample without B6O phase was obtained.

[0086] Using ethanol (purity>99%) as solvent and zirconium oxide balls as mixing medium, the weighed powders are mixed and mixed using a mixer at a mixing speed of 30-100rpm. After mixing for 12-36 hours, the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is crushed and sieved and poured into a graphite mold, and pressure sintered using a spark plasma sintering device. The entire process is carried out under vacuum.

[0087] The sintering process includes the following steps: room temperature to 450°C, the heating rate is 300°C / min, and the pressure applied to the sample is 5MPa. Then the pressure is increased to 60MPa within 2min. From 450°C to 1800°C, the heating rate is 300°C / min, and the pressure is 60MPa. After keeping at 1800°C for 5min, the pressure is reduced to 5MPa and heating is stopped, and the sample is cooled to room temperature with the furnace.

[0088] Compared with the sample without additives, the obtained sample is a pure boron sample without B6O phase. The relative density of pure boron block is 97.8%, Vickers hardness is 28-33GPa, three-point bending strength is 130-280MPa, and fracture toughness is 3-3.5MPa m 0.5 , the room temperature thermal conductivity is 20-30W / mK.

[0089] Example 5

[0090] Boron powder (purity of 95%, particle size of 0.1-5 μm) and boron-rich boron carbide (B6C particle size of 1-5 μm) are used as raw materials and the ingredients are prepared according to equation (8):

[0091] 98 B + 2 B2O3+ 6 B6C=138 B + 6 CO (8)

[0092] A pure boron sample without B6O phase was obtained.

[0093] Using ethanol (purity>99%) as solvent and zirconium oxide balls as mixing medium, the weighed powders are mixed and mixed using a mixer at a mixing speed of 30-100rpm. After mixing for 12-36 hours, the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is crushed and sieved and poured into a graphite mold, and pressure sintered using a spark plasma sintering device. The entire process is carried out under vacuum.

[0094] The sintering process includes the following steps: room temperature to 450°C, the heating rate is 300°C / min, and the pressure applied to the sample is 5MPa. Then the pressure is increased to 60MPa within 2min. From 450°C to 1800°C, the heating rate is 300°C / min, and the pressure is 60MPa. After keeping at 1800°C for 5min, the pressure is reduced to 5MPa and heating is stopped, and the sample is cooled to room temperature with the furnace.

[0095] Compared with the sample without additives, the obtained sample is a pure boron sample without B6O phase. The relative density of pure boron block is 98.8%, Vickers hardness is 30-35GPa, three-point bending strength is 140-300MPa, and fracture toughness is 3-3.5MPa m 0.5 , the room temperature thermal conductivity is 20-30W / mK.

[0096] Example 6

[0097] Boron powder (purity of 95%, particle size of 0.1-5 μm) and carbon black (particle size of 5-500 nm) are used as raw materials and the ingredients are prepared according to equation (9):

[0098] 98 B + 2 B2O3+ 6 C=102 B + 6 CO (9)

[0099] A pure boron sample without B6O phase was obtained.

[0100] Using ethanol (purity>99%) as solvent and zirconium oxide balls as mixing medium, the weighed powders are mixed and mixed using a mixer at a mixing speed of 30-100rpm. After mixing for 12-36 hours, the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is crushed and sieved and poured into a graphite mold, and pressure sintered using a spark plasma sintering device. The entire process is carried out under vacuum.

[0101] The sintering process includes the following steps: room temperature to 450°C, the heating rate is 300°C / min, and the pressure applied to the sample is 5MPa. Then the pressure is increased to 60MPa within 2min. From 450°C to 1800°C, the heating rate is 300°C / min, and the pressure is 60MPa. After keeping at 1800°C for 5min, the pressure is reduced to 5MPa and heating is stopped, and the sample is cooled to room temperature with the furnace.

[0102] Compared with the sample without additives, the obtained sample is a pure boron sample without B6O phase. The relative density of pure boron block is 99.1%, Vickers hardness is 30-35GPa, three-point bending strength is 160-300MPa, and fracture toughness is 3-3.5MPa m 0.5 , the room temperature thermal conductivity is 20-30W / mK.

[0103] Example 7

[0104] Boron powder (purity of 95%, particle size of 0.1-5 μm) and graphite (particle size of 0.5-100 μm) are used as raw materials and the ingredients are prepared according to equation (9):

[0105] 98 B + 2 B2O3+ 6 C=102 B + 6 CO (9)

[0106] A pure boron sample without B6O phase was obtained.

[0107] Using ethanol (purity>99%) as solvent and zirconium oxide balls as mixing medium, the weighed powders are mixed and mixed using a mixer at a mixing speed of 30-100rpm. After mixing for 12-36 hours, the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is crushed and sieved and poured into a graphite mold, and pressure sintered using a spark plasma sintering device. The entire process is carried out under vacuum.

[0108] The sintering process includes the following steps: room temperature to 450°C, the heating rate is 300°C / min, and the pressure applied to the sample is 5MPa. Then the pressure is increased to 60MPa within 2min. From 450°C to 1800°C, the heating rate is 300°C / min, and the pressure is 60MPa. After keeping at 1800°C for 5min, the pressure is reduced to 5MPa and heating is stopped, and the sample is cooled to room temperature with the furnace.

[0109] Compared with the sample without additives, the obtained sample is a pure boron sample without B6O phase. The relative density of pure boron block is 97.7%, Vickers hardness is 25-30GPa, three-point bending strength is 130-250MPa, and fracture toughness is 3-3.5MPa m 0.5 , the room temperature thermal conductivity is 20-30W / mK.

[0110] Example 8

[0111] Boron powder (purity of 95%, particle size of 0.1-5 μm) and B4C (particle size of 0.5-5 μm) are used as raw materials and the ingredients are prepared according to equation (6):

[0112] 98 B + 2 B2O3+ 6 B4C=126 B + 6 CO (6)

[0113] A pure boron sample without B6O phase was obtained.

[0114] Using ethanol (purity>99%) as solvent and zirconium oxide balls as mixing medium, the weighed powders are mixed and mixed using a mixer at a mixing speed of 30-100rpm. After mixing for 12-36 hours, the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is crushed and sieved and poured into a graphite mold, and pressure sintered using a spark plasma sintering device. The entire process is carried out under vacuum.

[0115] The sintering process includes the following steps: room temperature to 450°C, the heating rate is 300°C / min, and the pressure applied to the sample is 5MPa. From 450°C to 2000°C, the heating rate is 300°C / min, and the pressure is increased to 75MPa within 2 minutes after the temperature reaches 2000°C, and then kept at 2000°C for 10 minutes. After the insulation is completed, the pressure is reduced to 5MPa and the heating is stopped, and the sample is cooled to room temperature with the furnace.

[0116] Compared with the sample without additives, the obtained sample is a pure boron sample without B6O phase. The relative density of pure boron block is 99.1%, Vickers hardness is 31-35GPa, three-point bending strength is 150-300MPa, and fracture toughness is 3-3.5MPa m 0.5 , the room temperature thermal conductivity is 20-30W / mK.

[0117] Example 9

[0118] Boron powder (purity of 95%, particle size of 0.1-5 μm) and B4C (particle size of 0.5-5 μm) are used as raw materials and the ingredients are prepared according to equation (6):

[0119] 98 B + 2 B2O3+ 6 B4C=126 B + 6 CO (6)

[0120] A pure boron sample without B6O phase was obtained.

[0121] Using ethanol (purity>99%) as solvent and zirconium oxide balls as mixing medium, the weighed powders are mixed and mixed using a mixer at a mixing speed of 30-100rpm. After mixing for 12-36 hours, the resulting slurry is dried at 60-85°C by vacuum rotary evaporation. The dried powder is crushed and sieved and poured into a graphite mold, and pressure sintered using a spark plasma sintering device. The entire process is carried out under vacuum.

[0122] The sintering process includes the following steps: room temperature to 450°C, the heating rate is 200°C / min, and the pressure applied to the sample is 5MPa. From 450°C to 1800°C, the heating rate is 200°C / min, and then the temperature is kept at 1800°C for 5 minutes. After the heat preservation is completed, the heating is stopped and the sample is cooled to room temperature with the furnace.

[0123] Compared with the sample without additives, the obtained sample is a pure boron sample without B6O phase. The relative density of pure boron block is 97.5%, Vickers hardness is 28-31GPa, three-point bending strength is 150-250MPa, and fracture toughness is 3-3.5MPa m 0.5 , the room temperature thermal conductivity is 15-25W / mK.

[0124] In summary, by using commercial boron powder as raw material and adding additives such as boron carbide as deoxidizers, the oxygen in the starting boron powder can be effectively removed, thereby obtaining high-purity, high-hardness and high-density oxygen-free boron blocks.

[0125] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A high-purity, high-hardness and high-density oxygen-free boron block, characterized in that: Commercially available boron powder and boron carbide powder or a mixture of boron and carbon are used as raw materials, and the raw materials are mixed according to any one of the following chemical reaction equations (1) to (3): (100-y) B + y B2O3 + 3y B x C=(100+13y) B + 3y CO (1) (100-y) B + y B2O3 + 3y B4C=(100+13y) B + 3y CO (2) (100-y) B + y B2O3 + 3y C=(100+y) B + 3y CO (3) Among them, the value range of parameter x is: 4≤x≤10.5; the value range of parameter y is: 0≤y≤100.

2. The high-purity, high-hardness and high-density oxygen-free boron block according to claim 1, characterized in that: The carbon is graphite or carbon black.

3. The high-purity, high-hardness and high-density oxygen-free boron block according to claim 2, characterized in that: The purity of the graphite is greater than 99%, and the particle size is 0.5-100 μm; the purity of the carbon black is greater than 99%, and the particle size is 5-500 nm.

4. The high-purity, high-hardness and high-density oxygen-free boron block according to claim 1, characterized in that: The purity of the B4C is greater than 99%, and the particle size is 0.5-5 μm; when x=6, the purity of the B6C is greater than 99%, and the particle size is 1-5 μm.

5. A method for preparing a high-purity, high-hardness and high-density oxygen-free boron block as described in any one of claims 1 to 4, characterized in that: The preparation method comprises: Step 1, weighing raw material powders according to the proportion of the designed chemical reaction equation, mixing, drying and sieving the raw material powders; Step 2: Pour the raw material powder obtained in step 1 into a mold, and sinter it under pressureless sintering, hot pressing sintering or spark plasma sintering to obtain the required oxygen-free boron block.

6. The method for preparing a high-purity, high-hardness and high-density oxygen-free boron block according to claim 5, characterized in that: In the step 2, the sintering environment is a vacuum or flowing argon atmosphere.

7. The method for preparing a high-purity, high-hardness and high-density oxygen-free boron block according to claim 5, characterized in that: In the step 2, the sintering temperature ranges from 1600°C to 2000°C.

8. The method for preparing a high-purity, high-hardness and high-density oxygen-free boron block according to claim 5, characterized in that: In step 2, the insulation time ranges from 5 to 180 minutes.

9. The method for preparing a high-purity, high-hardness and high-density oxygen-free boron block according to claim 5, characterized in that: In the step 2, the loading pressure ranges from 5 to 75 MPa.

10. The method for preparing a high-purity, high-hardness and high-density oxygen-free boron block according to claim 5, characterized in that: In step 2, the heating rate ranges from 10 to 300° C. / min.

Citation Information

Patent Citations

  • Method for preparing superfine boron carbide powder by using combustion method

    CN101786624A

  • Purification of elemental boron

    GB1108290A

  • Boron carbide sintered compact and its production

    JP2000154062A

  • Method for manufacturing boron carbide

    JP2003277039A