Metal element and copper co-doped tungsten oxide powder and preparation method and application thereof
By adding yttrium, ytterbium or strontium and copper into tungsten oxide and reducing treatment, metal elements with high near-infrared and ultraviolet barrier properties were prepared and co-doped tungsten oxide powder with copper, solving the cost of existing energy-saving window materials. The problem of high and difficult to replace cesium has achieved cost-effective thermal insulation.
Patent Information
- Application Number
- CN202410951475.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
Existing energy-saving window materials are costly when achieving high near-infrared barrier and low visible light transmittance, and it is difficult to completely replace cesium. In strong light areas, low visible light transmittance, high UV barrier and high near-infrared shielding are required. The thermal insulation material is difficult to achieve.
By adding a specific content of yttrium, ytterbium or strontium and copper to a tungsten oxide, a metal element co-doped tungsten oxide powder is formed, and the infrared absorption performance of the material is enhanced by reducing treatment and cationic doping, and a cationic doping is prepared with Powders with high near-infrared barrier, ultraviolet barrier and suitable visible light transmittance.
It realizes cost-effective near-infrared and ultraviolet barrier functions, reduces material costs, and provides low-cost insulation solutions for building and automotive windows, which can replace some cesium tungsten bronze materials.
Smart Images

Figure CN118908279A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of thermal insulation materials, and more specifically, relates to a tungsten oxide powder co-doped with metal elements and copper, and a preparation method and application thereof. Background Art
[0002] With the proposal of my country's dual carbon goals, all walks of life are taking active actions. As a major energy consumer in society, the construction industry is under tremendous pressure. There are about 50 billion square meters of existing buildings in my country, and about 1 billion square meters of new buildings are added each year. Windows are the weak link in the building envelope. The energy consumed by windows accounts for about half of the energy consumed by the entire envelope, so they have great energy-saving potential. Car windows are also a channel for energy consumption. Therefore, the research and application of energy-saving window materials have become more and more popular in recent years.
[0003] In the solar spectrum, visible light and near infrared are the two largest parts of the solar spectrum energy, accounting for about 50% each. Visible light (280-780nm) is the basic source of indoor lighting, and near infrared (780-2500nm) is called heat ray, which has a significant heating effect and produces a strong sense of heat on human skin. Therefore, the main function of energy-saving window materials is to achieve visible light transmission and block near infrared rays that produce heat. Antimony tin oxide (ATO) and indium tin oxide (ITO) both have strong near-infrared blocking capabilities, but if ATO coating materials want to block 90% of near infrared rays, the amount of ATO added needs to be greatly increased, which means an increase in cost. When ITO coating materials achieve 90% near-infrared blocking, they have a higher visible light transmittance of 70-80%, but indium in ITO materials is a rare metal with a high price, which limits the large-scale application of ITO coating materials on windows.
[0004] Cesium tungsten oxide (Cs x WO3, also known as cesium tungsten bronze, is a near-infrared shielding material of cesium-modified tungsten oxide. It has been sought after by researchers and the market in recent years due to its high light transmittance of 70-80% and high near-infrared blocking rate of 85-95%, and its moderate price. There are many research and patents in this area. In recent years, with the rise in raw material prices, the price of cesium tungsten compounds has also been rising. The current market price of cesium compounds is 1.1 to 1.2 million yuan / ton, and the cost of cesium compounds accounts for more than 40% of the cost of cesium tungsten bronze, resulting in Cs xThe rise in the price of WO3. CN109678211A discloses a tantalum-doped cesium tungsten bronze and its preparation method and application. Tantalum is used to replace part of cesium, reducing the amount of cesium used. CN114853068A discloses a titanium-doped cesium tungsten bronze powder and its preparation method. The method of titanium-doped cesium tungsten oxide is used to reduce the amount of cesium used, which plays a certain role in reducing costs. Although the above patents reduce the amount of cesium used by doping with other metals, they still do not completely replace cesium. CN 107519889 B discloses a method for preparing a copper-doped tungsten trioxide composite nanofiber material. The copper doping greatly improves the photocatalytic degradation performance of tungsten trioxide, and also has excellent aniline degradation performance, which has great application prospects in the field of water pollution. The invention patent does not mention that the material has a near-infrared blocking function. Tan Dunqiang et al. (Study on the Preparation Process of Nano-tungsten Oxide Copper Composite Powder, Powder Metallurgy Technology, December 2007, 434-439) prepared a tungsten copper composite powder. The material was sintered in air atmosphere, and it was not mentioned that the material had near-infrared blocking function. Many existing technical solutions still focus on doping other metals with cesium to reduce the amount of cesium used. Some have achieved good results and reduced the amount of cesium used to a certain extent. Some have a much lower near-infrared blocking rate.
[0005] In addition, some areas with strong sunlight have shading requirements, especially thermal insulation materials with low visible light transmittance, high UV blocking rate and high near-infrared shielding rate are needed. However, due to the high visible light transmittance of cesium tungsten bronze, when used to prepare low-transmittance thermal insulation film, cesium tungsten bronze needs to be used with dark color paste for color adjustment, which further reduces the visible light transmittance of the thermal insulation film. Therefore, how to dope tungsten oxide with ordinary metals to make it have low transmittance, high UV blocking rate, near-infrared shielding rate and significantly reduce the price of modified tungsten oxide with infrared shielding function is the concern and pursuit of scientific researchers and the market. Summary of the invention
[0006] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a tungsten oxide powder co-doped with a metal element and copper.
[0007] Another object of the present invention is to provide a powder having near-infrared blocking function.
[0008] Another object of the present invention is to provide a method for preparing the metal element and copper co-doped tungsten oxide powder.
[0009] Another object of the present invention is to apply the tungsten oxide powder co-doped with the metal element and copper.
[0010] The above-mentioned purpose of this application is achieved through the following scheme:
[0011] A metal element and copper co-doped tungsten oxide powder, the chemical formula of which is A x Cu y WO3, wherein metal A is one of yttrium (Y), ytterbium (Yb) or strontium (Sr), x is 0.01 to 0.2, y is 0.05 to 0.4, Cu is copper, W is tungsten, and O is oxygen.
[0012] Preferably, x is 0.02 to 0.1.
[0013] Preferably, y is 0.15 to 0.25.
[0014] Tungsten trioxide is an n-type semiconductor material with a wide bandgap and a narrow bandgap (2.5-2.8 eV). A large number of studies have shown that the surface plasmon resonance of semiconductor materials can absorb light of a specific wavelength. In this application, metal A and copper are co-doped into tungsten oxide and reduced to obtain a powder with infrared blocking function. Reduction treatment of tungsten oxide nanoparticles and the addition of other cations can accumulate a large number of free electrons on their surface, so that they have the characteristic of absorbing infrared light through plasma resonance. Secondly, the reduction treatment and cations can distort the tungsten oxide lattice, generate oxygen vacancies and lattice defects, and then generate free electrons, which enhances the polaron absorption, thereby improving the infrared absorption performance of the material.
[0015] The present invention also protects a powder having a near-infrared blocking function, wherein the chemical formula of the powder having a near-infrared blocking function is A x Cu y WO3, wherein metal A is one of yttrium Y, ytterbium Yb or strontium Sr, x is 0.01 to 0.2, and y is 0.05 to 0.4.
[0016] The present invention also protects a method for preparing the above-mentioned metal element and copper co-doped tungsten oxide powder, comprising the following steps:
[0017] S1. Adding a tungsten source, a copper source, and a metal A source to water and stirring to obtain a first mixture;
[0018] S2. subjecting the first mixture to a hydrothermal reaction to separate and obtain a second mixture;
[0019] S3. calcining the second mixture under a reducing atmosphere to obtain tungsten oxide powder co-doped with the metal element and copper.
[0020] Preferably, the tungsten source is one or more of ammonium metatungstate, ammonium paratungstate or tungstic acid.
[0021] Preferably, the copper source is copper oxide and / or copper salt.
[0022] More preferably, the copper source is one or more of basic copper carbonate, copper oxide, cuprous oxide, copper sulfate, cupric chloride or copper acetate. More preferably, the copper source is basic copper carbonate or cuprous oxide.
[0023] Preferably, the metal A source is an oxide of metal A and / or a salt of metal A.
[0024] More preferably, the metal A source is one or more of yttrium carbonate, yttrium oxide, yttrium hydroxide, ytterbium carbonate, ytterbium oxide, ytterbium nitrate, strontium carbonate, strontium oxide, strontium sulfate, strontium oxalate or strontium nitrate. More preferably, the metal A source is one or more of yttrium carbonate, yttrium oxide, ytterbium carbonate, ytterbium oxide, strontium carbonate or strontium oxide.
[0025] Preferably, the stirring time in step S1 is 2 to 12 hours. More preferably, the stirring time in step S1 is 8 to 12 hours.
[0026] Preferably, the temperature of the hydrothermal reaction in step S2 is 180-260° C. More preferably, the temperature of the hydrothermal reaction in step S2 is 200-220° C.
[0027] Preferably, the hydrothermal reaction time in step S2 is 2 to 48 hours. More preferably, the hydrothermal reaction time in step S2 is 12 to 48 hours.
[0028] Preferably, the separation method in step S2 is one or more of decantation, filtration, and centrifugation. More preferably, the separation method in step S2 is centrifugation.
[0029] Preferably, the reducing atmosphere in step S3 is a mixture of H2 and N2. More preferably, the reducing atmosphere is a mixture of 5% H2 and 95% N2.
[0030] Preferably, the calcination temperature in step S3 is 500-900° C. More preferably, the calcination temperature in step S3 is 700-800° C.
[0031] Preferably, the calcination holding time in step S3 is 1 to 6 hours. More preferably, the calcination holding time in step S3 is 3 to 5 hours.
[0032] The present invention also protects the use of the above metal element and copper co-doped tungsten oxide powder in the preparation of thermal insulation materials.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The present invention forms a tungsten oxide powder doped with metal elements and copper by adding a specific content of metal A and copper into tungsten oxide, which has a high near-infrared blocking rate, ultraviolet blocking rate and suitable visible light transmittance, and can be used as a substitute for cesium tungsten bronze with lower visible light transmittance; and has the advantage of low price. The tungsten oxide doped with metal elements and copper in the present invention is conducive to the application of thermal insulation materials in buildings and automobile side windows, and provides a cost-effective product for my country's energy conservation and emission reduction work. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a picture of the finished product of Example 3 (1-2) and Example 4 (1-3) coated on glass.
[0036] Figure 2 This is the XRD pattern of Comparative Example 1.
[0037] Figure 3 This is the XRD diagram of Example 1. DETAILED DESCRIPTION
[0038] The content of the present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present embodiment are conventional reagents, methods and equipment in the art.
[0039] Example 1
[0040] A metal element and copper co-doped tungsten oxide powder, the chemical formula is Y 0.1 Cu 0.2 WO3, the preparation method thereof comprises the following steps:
[0041] S1. Add 14.27 g yttrium carbonate, 19.1 g basic copper carbonate, 200 g tungstic acid, 280 g deionized water, and place in a beaker and stir for 8 hours.
[0042] S2. The obtained water mixture is placed in a small hydrothermal reactor and kept at 200°C for 15 hours; the mixture after the hydrothermal reaction is placed in an oven and baked at 100°C until dry.
[0043] S3. The yttrium copper tungsten mixture is placed in a rotary atmosphere furnace for calcination in a reducing atmosphere (hydrogen H2, 5%, nitrogen N2, 95%) at a temperature of 700°C for 4 hours. The sintered yttrium copper tungsten oxide is crushed by a pulverizer and dried for later use.
[0044] Example 2
[0045] A metal element and copper co-doped tungsten oxide powder, the chemical formula is Y 0.05 Cu0.2 WO3, the preparation method thereof comprises the following steps:
[0046] S1. Add 10.9 g yttrium carbonate, 4.4 g cuprous oxide, 198.4 g ammonium metatungstate, 280 g deionized water, and place in a beaker and stir for 8 hours.
[0047] S2. The obtained water mixture is placed in a small hydrothermal reactor and kept at 200°C for 15 hours; the mixture after the hydrothermal reaction is placed in an oven and baked at 100°C until dry.
[0048] S3. The yttrium copper tungsten mixture is placed in a rotary atmosphere furnace for sintering in a reducing atmosphere (hydrogen H2, 5%, nitrogen N2, 95%) at a temperature of 700°C for 4 hours. The sintered yttrium copper tungsten oxide is crushed by a pulverizer and dried for later use.
[0049] Example 3
[0050] A metal element and copper co-doped tungsten oxide powder, the chemical formula is Yb 0.02 Cu 0.15 WO3, the preparation method thereof comprises the following steps:
[0051] S1. Add 280g of deionized water to 2.9g of ytterbium carbonate, 14.4g of basic copper carbonate, and 209g of ammonium paratungstate, and place in a beaker and stir for 10 hours.
[0052] S2. The obtained water mixture is placed in a small hydrothermal reactor and kept at 180°C for 24 hours; the mixture after the hydrothermal reaction is placed in an oven and baked at 100°C until dry.
[0053] S3. The ytterbium copper tungsten mixture is placed in a rotary atmosphere furnace for sintering in a reducing atmosphere (hydrogen H2, 5%, nitrogen N2, 95%) at a temperature of 750°C for 3 hours. The sintered ytterbium copper tungsten oxide is crushed by a pulverizer and dried for later use.
[0054] Example 4
[0055] A metal element and copper co-doped tungsten oxide powder, the chemical formula is Yb 0.05 Cu 0.2 WO3, the preparation method thereof comprises the following steps:
[0056] S1. Add 10.9 g of ytterbium carbonate, 4.4 g of cuprous oxide, and 198.4 g of ammonium metatungstate to 280 g of deionized water and place in a beaker and stir for 8 hours.
[0057] S2. The obtained water mixture is placed in a small hydrothermal reactor and kept at 200°C for 15 hours; the mixture after the hydrothermal reaction is placed in an oven and baked at 100°C until dry.
[0058] S3. The ytterbium copper tungsten mixture is placed in a rotary atmosphere furnace for sintering in a reducing atmosphere (hydrogen H2, 5%, nitrogen N2, 95%) at a temperature of 700°C for 4 hours. The sintered ytterbium copper tungsten oxide is crushed by a pulverizer and dried for later use.
[0059] Example 5
[0060] A metal element and copper co-doped tungsten oxide powder, the chemical formula is Sr 0.05 Cu 0.2 WO3, the preparation method thereof comprises the following steps:
[0061] S1. 5.9 g strontium carbonate, 4.4 g cuprous oxide, 199 g ammonium metatungstate, add 280 g deionized water, place in a beaker and stir for 6 hours.
[0062] S2. The obtained water mixture is placed in a small hydrothermal reactor and kept at 210°C for 12 hours; the mixture after the hydrothermal reaction is placed in an oven and baked at 100°C until dry.
[0063] S3. The strontium copper tungsten mixture is placed in a rotary atmosphere furnace for sintering in a reducing atmosphere (hydrogen H2, 5%, nitrogen N2, 95%) at a temperature of 800°C for 3 hours. The sintered strontium copper tungsten oxide is crushed by a pulverizer and dried for later use.
[0064] Comparative Example 1
[0065] A copper-doped tungsten oxide powder, the chemical formula is Cu 0.2 WO3, the preparation method thereof comprises the following steps:
[0066] S1. Add 19.1 g of basic copper carbonate and 200 g of ammonium metatungstate to 280 g of deionized water and place in a beaker and stir for 8 hours.
[0067] S2. The obtained water mixture is placed in a hydrothermal reactor and kept at 200°C for 10 hours; the mixture after the hydrothermal reaction is placed in an oven and baked at 100°C until dry.
[0068] S3. The copper-tungsten mixture is placed in a rotary atmosphere furnace for sintering in a reducing atmosphere (hydrogen H2, 5%, nitrogen N2, 95%) at a temperature of 750°C for 2 hours. The sintered copper-tungsten oxide is crushed by a pulverizer and dried for later use.
[0069] Comparative Example 2
[0070] A cesium-doped tungsten oxide powder is prepared by the preparation method disclosed in Example 2 of CN107915257A.
[0071] Performance Testing
[0072] The optical properties of the powder are characterized as follows:
[0073] Take 60g of modified tungsten oxide powder A x Cu y WO3, 30g dispersant, 110g ethyl acetate solvent, added to the ball mill for dispersion (speed 300 rpm), after 48 hours of ball milling, taken out for use. Take pressure sensitive adhesive PSA 10g, ethyl acetate 10g, modified tungsten oxide dispersion 6g and mix them evenly, and use a 50 micron wet film scraper to make a film on 5mm ordinary glass, and use a solar film detector to test its optical properties. The results are shown in Table 1.
[0074] Table 1 Ultraviolet blocking rate, near infrared blocking rate and visible light transmittance of the embodiments and comparative examples
[0075] Example UV blocking rate (%) Near infrared blocking rate (%) Visible light transmittance (%) Example 1 84.1 96.3 38.8 Example 2 81.2 92.4 46.7 Example 3 85.3 90.2 47.8 Example 4 75.3 82.6 57.8 Example 5 86.1 93.1 45.6 Comparative Example 1 39.1 80.6 53.9 Comparative Example 2 52.0 90.1 74.0
[0076] From the above Table 1, it can be seen that the metal A and copper co-doped tungsten oxide powder A of the present invention x Cu y WO3 has an ultraviolet light blocking rate of 75.3% to 86.1%, a near infrared blocking rate of 82.6% to 96.3%, and a visible light transmittance of 38.8% to 57.8%.
[0077] In the two comparative examples, the UV blocking rates were 39.1% and 52.0% respectively, the near-infrared blocking rates were 80.6% and 90.1% respectively, and the visible light transmittances were 53.9% and 74.0% respectively, which cannot simultaneously meet the requirements of high UV blocking rate, high near-infrared blocking rate and low visible light transmittance.
[0078] Figure 2 This is the XRD diagram of comparative example 1. Comparative example 1 is copper-doped tungsten oxide. From the diffraction spectrum analysis, it is found that the compound is well consistent with the standard tungsten oxide spectrum, and the diffraction peaks corresponding to 35°, 40°, and 50° are well consistent with the standard diffraction spectrum of copper oxide. Figure 3 This is the XRD diagram of Example 1. Example 1 is tungsten oxide doped with yttrium copper. From the diffraction spectrum analysis, it is found that the compound is well matched with the standard tungsten oxide spectrum, and the diffraction peaks corresponding to 35°, 40°, and 50° are well matched with the standard diffraction spectrum of copper oxide. Compared with the standard yttrium oxide diffraction spectrum, it is found that 20°, 30°, 50°, and 60° all have corresponding diffraction peaks, but the peak intensity is relatively low, corresponding to the low yttrium doping amount. The diffraction peak intensity of Example 1 is stronger than that of Comparative Example 1, which means that Example 1 has a high degree of crystallinity.
[0079] The above embodiments of the present invention are only for clearly illustrating the present invention, and are not intended to limit the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.
Claims
1. A tungsten oxide powder co-doped with a metal element and copper, characterized in that: The chemical formula of the metal element and copper co-doped tungsten oxide powder is A x Cu y WO3, wherein metal A is one of yttrium Y, ytterbium Yb or strontium Sr, x is 0.01 to 0.2, and y is 0.05 to 0.
4.
2. The tungsten oxide powder co-doped with metal elements and copper according to claim 1, characterized in that: x is 0.02~0.1, and y is 0.15~0.
25.
3. A powder with near-infrared blocking function, characterized in that: The chemical formula of the powder having near infrared blocking function is A x Cu y WO3, wherein metal A is one of yttrium Y, ytterbium Yb or strontium Sr, x is 0.01 to 0.2, and y is 0.05 to 0.
4.
4. A method for preparing the metal element and copper co-doped tungsten oxide powder according to claim 1-2, characterized in that: The following steps are involved: S1. Adding a tungsten source, a copper source, and a metal A source to water and stirring to obtain a first mixture; S2. subjecting the first mixture to a hydrothermal reaction to separate and obtain a second mixture; S3. calcining the second mixture under a reducing atmosphere to obtain tungsten oxide powder co-doped with the metal element and copper.
5. The preparation method according to claim 2, characterized in that: The tungsten source is one or more of ammonium metatungstate, ammonium paratungstate or tungstic acid.
6. The preparation method according to claim 2, characterized in that: The copper source is copper oxide and / or copper salt.
7. The preparation method according to claim 2, characterized in that: The metal A source is a metal A oxide and / or a metal A salt.
8. The preparation method according to claim 2, characterized in that: The temperature of the hydrothermal reaction in step S2 is 180-260°C.
9. The preparation method according to claim 2, characterized in that: The reducing atmosphere in step S3 is a mixed gas of H2 and N2.
10. Use of the metal element and copper co-doped tungsten oxide powder according to claim 1 in the preparation of thermal insulation materials.