Zinc-doped ultrahigh-nickel ternary lithium ion battery positive electrode material as well as preparation method and application thereof

Through ALD technology, ZnO is deposited on the surface of nickel-cobalt-manganese ternary precursor and mixed with lithium salt to calcinate it, and the positive electrode material of zinc-doped ultra-high nickel ternary lithium-ion battery was prepared, solving the material stability caused by the increase in nickel content in lithium-ion batteries. The cyclic stability and electrochemical properties of the material are improved.

CN118908298AActive Publication Date: 2024-11-08NANJING UNIV OF AERONAUTICS & ASTRONAUTICS

Patent Information

Application Number
CN202410852521.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-08
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

When the nickel content of the existing ultra-high nickel ternary lithium-ion battery cathode material increases, the residual lithium compound on the surface of the material increases, affecting thermal stability and cycling performance. The existing doping methods have zinc elements inhomogeneity, which affects the material. Cyclic stability.

Method used

ZnO is uniformly deposited on the surface of nickel-cobalt-manganese ternary precursor by bottom-up chemical vapor deposition (ALD) technology, and mixed with lithium salt and calcined at high temperature to prepare zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode. Materials, this method controls the molar dose ratio of zinc, reduces heterophasic phase formation, and improves the crystal structure and cyclic electrochemical properties of the material.

Benefits of technology

The better crystal structure and cyclic electrochemical performance of the positive electrode material of zinc-doped ultra-high nickel ternary lithium-ion battery is achieved, avoiding the waste of energy substances caused by excessive processes, and enhancing the cyclic stability and safety performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908298A_ABST
    Figure CN118908298A_ABST
Patent Text Reader

Abstract

The invention discloses a zinc-doped ultrahigh-nickel ternary lithium ion battery positive electrode material as well as a preparation method and application thereof. The preparation method comprises the following steps: by taking Zn salt and water as raw materials, coating ZnO on the surface of a nickel-cobalt-manganese ternary precursor through ALD (Atomic Layer Deposition), mixing the obtained precursor with lithium salt, and carrying out high-temperature calcination to finally obtain the Zn-doped ultrahigh-nickel ternary lithium ion battery positive electrode material. According to the preparation method provided by the invention, the crystal structure of the material is stabilized by virtue of the Zn element in the shell and the bulk phase, and the collapse of the material structure in a long-term circulation process is avoided, so that the comprehensive electrochemical performance of the material is improved, and the application prospect is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a zinc-doped ultra-high nickel ternary lithium ion battery positive electrode material and a preparation method and application thereof. Background Art

[0002] Energy conservation and new energy vehicles, and new energy storage have become key areas of national investment and development. Stimulated by multiple factors such as continuous breakthroughs in key technologies and dividends from industrial policies, the business of power batteries and energy storage batteries has flourished like wildfire. my country's lithium industry is showing a booming development trend. The growing demand for high-energy, high-power density lithium-ion batteries has triggered great research interest in high-performance positive electrode materials. The positive electrode materials of the next generation of lithium-ion batteries need to have higher energy density, longer cycle life and better safety characteristics, suitable for electric vehicles and stationary energy storage applications. Ternary LiNixCoyMnzO2 (X+Y+Z=1) is generally considered to be the most promising alternative after LiFePO4 and LiCoO2.

[0003] Among various possible compositions, ultra-high nickel ternary LiNi x Co y Mn z O2 (x>0.9) is widely valued for its high energy density and cost-effectiveness. Unfortunately, as the nickel content increases, the residual lithium compounds on the surface of the material will increase. During the preparation of the positive electrode sheet, excessive residual lithium will cause the slurry to gel. In addition, the residual lithium compounds will aggravate the gas precipitation during the battery charging and discharging process, resulting in reduced thermal stability of the positive electrode material and capacity attenuation. Ultra-high nickel content will also cause irreversible phase changes, resulting in poor cycle performance of the material.

[0004] In order to solve these problems, surface coating, lattice doping, core-shell preparation, concentration gradient structure, single crystal materials, etc. can be used to improve the structural stability and electrochemical performance of the materials. By doping with multivalent single dopants (such as Al, Ti, Zr, Mg, Mo, Sn, B, V, W, Cr), several key harmful factors such as gradual phase change, voltage decay, electrolyte degradation and transition metal (TMs) dissolution can be effectively alleviated. The incorporation of these ions greatly improves the cycle stability, but reduces the capacity of the positive electrode material.

[0005] Doping the ultra-high nickel ternary positive electrode material with the metal element Zn can solve its shortcomings to a certain extent, improve the cycle stability and safety performance of the ultra-high nickel ternary positive electrode material, and improve the electrochemical performance of the positive electrode material.

[0006] CN107994227A discloses a method of using a coprecipitation method to use a Na2CO3 solution as a precipitant to coprecipitate a mixed solution of NiSO4, CoSO4 and MnSO4 with ZnSO4 to obtain a Zn-doped Ni 0.5 Co 0.2 Mn 0.3 (OH)2 type ternary material precursor. This method has a simple process and the product has a high tap density, but the Zn element doped by this method is uneven, which will affect the cycle stability of the positive electrode material.

[0007] CN 115676913A discloses a method for preparing a core-shell structure ultra-high nickel ternary precursor by doping layered basic zinc carbonate crystals. The method improves the cycle stability of the positive electrode material, increases the cycle life, and improves the safety performance and electrochemical performance of the positive electrode material. However, the precursor prepared by the method is Ni 0.8 Co 0.1 Mn 0.1 (OH)2 type, and no research has been conducted on materials with even higher nickel content (Ni ≥ 0.9). Summary of the invention

[0008] In view of the deficiencies in the prior art, the object of the present invention is to provide a zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material and a preparation method and application thereof.

[0009] In order to solve the problems of the prior art, the technical solution adopted by the present invention is:

[0010] A method for preparing a zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material, using Zn salt and water as raw materials, coating ZnO on the surface of a nickel-cobalt-manganese ternary precursor by ALD, and then mixing it with a lithium salt, and calcining it at high temperature to finally obtain a Zn-doped ultra-high nickel ternary lithium-ion battery positive electrode material.

[0011] The method for preparing the zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material comprises the following steps:

[0012] Step 1, placing the dried nickel-cobalt-manganese ternary precursor powder on the ALD sample tray, using 10-25°C H2O as the oxidant of the Zn source, and selecting high-purity argon as the carrier gas and process purge gas, the temperature of the reaction outer chamber is set to 210°C, and the temperature of the inner chamber is set to 200°C. During deposition, first, the Zn source pulse is 150ms, wait for 10s, purge argon for 10s, wait for 5s, then pulse H2O for 100ms, wait for 5s, purge argon for 10s, and finally wait for 5s to enter the next cycle; after the set number of cycles, a ternary precursor with surface deposited ZnO is obtained;

[0013] Step 2: Take the deposited ZnO ternary precursor and mix it evenly with LiOH·H2O, and calcine it in stages in a tubular atmosphere furnace with flowing oxygen, first keep it at 450-550°C for 4-6 hours, then keep it at 600-800°C for 12-16 hours, and finally cool it to room temperature with the furnace, grind and sieve to obtain zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material.

[0014] Preferably, the chemical formula of the ultra-high nickel ternary precursor is Ni 0.90 Co 0.05 Mn 0.05 (OH)2, the zinc source is diethyl zinc, and the lithium source is at least one of lithium nitrate, lithium acetate, lithium carbonate and lithium hydroxide.

[0015] Preferably, the vacuum drying temperature of the nickel-cobalt-manganese ternary precursor powder is 60-100°C.

[0016] Preferably, the vacuum drying temperature of the ternary precursor powder is 80°C.

[0017] Preferably, the mass of the dried nickel-cobalt-manganese ternary precursor powder placed in the ALD sample tray is 2g-4g.

[0018] Preferably, the number of ALD cycles is 25-200 times.

[0019] Preferably, the Ni of the dried nickel-cobalt-manganese ternary precursor powder is 0.90 Co 0.05 Mn 0.05 The mass ratio of (OH)2 to LiOH·H2O is 0.95:0.46.

[0020] Preferably, the powder is sieved after grinding in step 2, and the mesh size of the sieve is 300 meshes.

[0021] The zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material prepared by the above preparation method has Ni≥0.9 mol, and its diffraction peak is a characteristic peak of a-NaFeO2 layered structure, belonging to the hexagonal crystal system and R-3m space group.

[0022] The zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material prepared by the above preparation method is used as a positive electrode in a lithium-ion battery.

[0023] Beneficial effects:

[0024] Compared with the prior art, the present invention proposes to use the ALD method to deposit uniform ZnO on the surface of the nickel-cobalt-manganese ternary precursor. On the one hand, the addition of zinc ions by molar dosage ratio can effectively control the molar dosage ratio of zinc in the material, reduce the influence of excessive zinc incorporation on the material morphology and crystal structure, and is conducive to the precise regulation of the material synthesis process and element ratio. At the same time, it can avoid the formation of impurities to a certain extent, which is conducive to the accurate judgment and analysis of the influence of zinc ions on material properties and structure; on the other hand, zinc ions are directly embedded into a single metal oxide through one-step sintering, which is conducive to the preparation of layered positive electrode materials with low cation mixing degree and good crystal structure, avoiding the breakage of some ternary positive electrode material precursor particles and the waste of energy substances caused by too many cumbersome processes. Therefore, the zinc-doped ultra-high nickel ternary lithium ion battery positive electrode materials prepared by the ALD method proposed by the present invention show better crystal structure and cycle electrochemical performance than those prepared by other methods.

[0025] The present invention can also avoid the mutual inhibition of the two precursors on the material morphology during the in-situ synthesis process, reduce the influencing factors of the controllable synthesis of the material, maintain the morphology of the single metal oxide to a certain extent, and can be applied to other applied research in the field of electrochemical energy or photocatalytic material synthesis. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 XRD diagrams of Examples 1 to 3 and Comparative Examples 1 to 10 of the present invention;

[0027] Figure 2 is the SEM image of Example 2;

[0028] Figure 3 It is the SEM picture of comparative example 1;

[0029] Figure 4 is the EDS diagram of Example 2;

[0030] Figure 5 The cycle performance curves of Examples 1 to 3 and Comparative Examples 1 to 4 are shown. DETAILED DESCRIPTION

[0031] In view of the deficiencies in the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. That is, based on the research of the prior art, the present invention proposes an ALD method to deposit uniform ZnO on the surface of the nickel-cobalt-manganese ternary precursor. On the one hand, the addition of zinc ions by molar dosage ratio can effectively control the molar dosage ratio of zinc in the material, reduce the influence of excessive zinc incorporation on the material morphology and crystal structure, and is conducive to the precise regulation of the material synthesis process and element ratio. At the same time, it can avoid the formation of impurities to a certain extent, which is conducive to the accurate judgment and analysis of the influence of zinc ions on material properties and structure; on the other hand, zinc ions are directly embedded into a single metal oxide through one-step sintering, which is conducive to avoiding the waste of energy and materials due to too many cumbersome processes.

[0032] The technical scheme of the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise specified, the equipment and reagents used in the present invention are conventional commercial products in the field of this technology. The room temperature proposed in the present invention refers to 25°C.

[0033] The technical solution, its implementation process and principle will be further explained as follows.

[0034] A method for preparing a zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material comprises the following steps:

[0035] Step 1, placing the dried nickel-cobalt-manganese ternary precursor powder on the ALD sample tray, using 10-25°C H2O as the oxidant of the Zn source, and selecting high-purity argon as the carrier gas and process purge gas, the temperature of the reaction outer chamber is set to 210°C, and the temperature of the inner chamber is set to 200°C. During deposition, first, the Zn source pulse is 150ms, wait for 10s, purge argon for 10s, wait for 5s, then pulse H2O for 100ms, wait for 5s, purge argon for 10s, and finally wait for 5s to enter the next cycle; after the set number of cycles, a ternary precursor with surface deposited ZnO is obtained;

[0036] Step 2: Take the deposited ZnO ternary precursor and mix it evenly with LiOH·H2O, and calcine it in stages in a tubular atmosphere furnace with flowing oxygen, first keep it at 450-550°C for 4-6 hours, then keep it at 600-800°C for 12-16 hours, and finally cool it to room temperature with the furnace, grind and sieve to obtain zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material.

[0037] In the present invention, the vacuum drying temperature of the ternary precursor powder is 60-100° C., preferably 80° C. The staged sintering lithiation process is 500° C. for 4.5-5.5 hours, then 650° C.-800° C. for 13-15 hours. In a preferred embodiment, the sintering process is first 500° C. for 5 hours, then 700° C. for 14 hours.

[0038] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0039] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0040] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0041] Embodiment 1:

[0042] Weigh 2.00g Ni 0.90 Co 0.05 Mn 0.05 (OH)2 powder was placed in the ALD sample tray, diethyl zinc was used as the zinc source, H2O at room temperature was used as the oxidant of the Zn source, and high-purity argon was selected as the carrier gas and process purge gas. The temperature of the reaction chamber was set to 210°C, and the temperature of the inner chamber was set to 200°C. During the reaction, a sub-cycle of each source was: Zn source pulse time 150ms, H2O source pulse time 100ms, after 10s of Zn source, 10s of argon purge, wait 5s, then enter H2O, and then 10s of argon purge, and then wait 5s to enter the next cycle. After 25 cycles, a ternary precursor with uniformly deposited ZnO was obtained. 0.95 g of the ternary precursor powder was weighed and evenly mixed with 0.46 g of LiOH·H2O, wherein nLi:n(Ni+Co+Mn+Zn)=1.05:1 (molar ratio). The precursor was placed in an oxygen-permeable tubular furnace for staged sintering, first at 500°C for 5 h, then at 700°C for 14 h, and finally cooled to room temperature with the furnace. The zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material was obtained by grinding and sieving. The test results of button batteries made using the material are shown in Table 1.

[0043] Embodiment 2:

[0044] Except that the number of cycles was changed from 25 to 50, the rest was the same as in Example 1.

[0045] Embodiment 3:

[0046] Except that the number of cycles was changed from 25 to 100, the rest was the same as in Example 1.

[0047] Comparative Example 1:

[0048] Weigh 0.95g Ni 0.90 Co 0.05 Mn 0.05 (OH)2 was uniformly mixed with 0.46g LiOH·H2O, wherein nLi:n(Ni+Co+Mn)=1.05:1 (molar ratio), and the mixture was placed in an oxygen-permeable tubular furnace for staged sintering, first at 500°C for 5h, then at 700°C for 14h, and finally cooled to room temperature with the furnace, and ground and sieved to obtain a zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material. The test results of button batteries made using the material are shown in Table 1.

[0049] Comparative Example 2:

[0050] Weigh 3.76g Ni 0.90 Co 0.05 Mn 0.05 (OH)2 and 0.03g ZnO and 1.74g LiOH·H2O powder were ball-milled for 15min, wherein nLi:n(Ni+Co+Mn+Zn)=1.05:1 (molar ratio), and then placed in an oxygen-permeable tubular furnace for staged sintering, first at 500℃ for 5h, then at 700℃ for 14h, and finally cooled to room temperature with the furnace, ground and sieved to obtain zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material. The test results of button batteries made with the material are shown in Table 1. (ZnO-1)

[0051] Comparative Example 3:

[0052] Weigh 3.72g Ni 0.90 Co 0.05 Mn 0.05 (OH)2 and 0.07g ZnO and 1.74g LiOH·H2O powder were ball-milled for 15min, wherein nLi:n(Ni+Co+Mn+Zn)=1.05:1 (molar ratio), and then placed in an oxygen-permeable tubular furnace for staged sintering, first at 500℃ for 5h, then at 700℃ for 14h, and finally cooled to room temperature with the furnace, ground and sieved to obtain zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material. The test results of button batteries made with the material are shown in Table 1. (ZnO-2)

[0053] Comparative Example 4:

[0054] Weigh 3.60g Ni 0.90 Co 0.05 Mn 0.05(OH)2 and 0.17g C2H4O6Zn and 1.73g LiOH·H2O powder were ball-milled for 15min, wherein nLi:n(Ni+Co+Mn+Zn)=1.05:1 (molar ratio), and then placed in an oxygen-permeable tubular furnace for staged sintering, first at 500℃ for 5h, then at 700℃ for 14h, and finally cooled to room temperature with the furnace, ground and sieved to obtain zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material. The test results of button batteries made with the material are shown in Table 1. (ZnO-5)

[0055] The positive electrode materials obtained in the above-mentioned Examples 1 to 3 and Comparative Examples 1 to 4 were made into 2032-type button-type simulated batteries to test their electrochemical performance. The specific steps are as follows: (1) The above-mentioned positive electrode materials, conductive acetylene black and polyvinylidene fluoride (PVDF) were weighed in a mass ratio of 8:1:1, and PVDP was first dissolved in an appropriate amount of N-methylpyrrolidone (NMP), and then the mixed positive electrode materials and acetylene black powder were added to NMP and stirred to form a slurry; (2) The slurry was evenly scraped on the aluminum foil substrate, the wet electrode was placed in a vacuum drying oven, dried at 110°C for 12 hours, and cut into positive electrode sheets; (3) In a dry glove box, a simulated battery was assembled. The above-mentioned homemade positive electrode sheet was used as the positive electrode, the metal lithium sheet was used as the negative electrode, the Celgard2500 membrane was used as the diaphragm, and the electrolyte was 1 mol·L -1 The LiPF6 was dissolved in a solution of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) (volume ratio 1:1:1) to test its electrochemical properties, as shown in Table 1.

[0056] Table 1 Electrochemical performance of positive electrode materials of Examples 1-3 and Comparative Examples 1-4 at 2.70-4.55V

[0057]

[0058] It can be seen from Table 1 that after Zn doping modification by ALD method, the first discharge specific capacity is improved. The discharge specific capacity of Example 2 at 0.1C reaches 246.6 mAh·g -1 , and has the highest first charge and discharge efficiency, indicating that zinc doping improves the deintercalation ability of lithium ions. The first charge and discharge efficiencies of Comparative Examples 2 to 4 are much lower than those of Examples 1 to 3 and Comparative Example 1, which is due to particle breakage caused by ball milling. In addition, their capacity retention rates after 100 cycles are also lower than those of the sample in the embodiment. In addition to the reason of particle breakage, it is also due to the uneven distribution of zinc ions in the material. It can be seen that compared with the method of solid-phase sintering after ball milling, the positive electrode material obtained by the ALD coating method has better cycle stability.

[0059] Comparative Example 5:

[0060] Weigh 3.76g Ni0.90 Co 0.05 Mn 0.05 (OH)2, 0.08g C2H4O6Zn and 1.74g LiOH·H2O powder and 0.4g PVP were added to 20mL ethanol, wherein nLi:n(Ni+Co+Mn+Zn)=1.05:1 (molar ratio). After heating in a water bath at 80°C with stirring for 2h, the mixture was dried in a vacuum oven at 80°C and sintered in sections in an oxygen-permeable tubular furnace. The mixture was first kept at 500°C for 5h and then at 700°C for 14h. The mixture was finally cooled to room temperature with the furnace and ground and sieved to obtain a zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material.

[0061] (Zinc-1 Acetate)

[0062] Comparative Example 6:

[0063] Weigh 3.72g Ni 0.90 Co 0.05 Mn 0.05 (OH)2, 0.16g C2H4O6Zn and 1.74g LiOH·H2O powder and 0.4g PVP were added to 20mL ethanol, wherein nLi:n(Ni+Co+Mn+Zn)=1.05:1 (molar ratio). After heating in a water bath at 80°C with stirring for 2h, it was vacuum dried at 80°C and sintered in an oxygen-permeable tubular furnace in stages, first at 500°C for 5h, then at 700°C for 14h, and finally cooled to room temperature with the furnace, and ground and sieved to obtain zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material.

[0064] (Zinc-2 Acetate)

[0065] Comparative Example 7:

[0066] Weigh 3.60g Ni 0.90 Co 0.05 Mn 0.05 (OH)2, 0.39g C2H4O6Zn and 1.73g LiOH·H2O powder and 0.4g PVP were added to 20mL ethanol, wherein nLi:n(Ni+Co+Mn+Zn)=1.05:1 (molar ratio). After heating in a water bath at 80°C with stirring for 2h, the mixture was vacuum dried at 80°C and sintered in stages in an oxygen-permeable tubular furnace, first at 500°C for 5h, then at 700°C for 14h, and finally cooled to room temperature with the furnace, and ground and sieved to obtain zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material.

[0067] (Zinc-5 Acetate)

[0068] Comparative Example 8:

[0069] Weigh 3.76g Ni 0.90 Co0.05 Mn 0.05 (OH)2, 0.12g Zn(NO3)2·6H2O and 1.74g LiOH·H2O powder and 0.4g PVP were added to 20mL ethanol, wherein nLi:n(Ni+Co+Mn+Zn)=1.05:1 (molar ratio), heated in a water bath at 80℃ and stirred for 2h, then dried in vacuum at 80℃, and sintered in sections in an oxygen-permeable tubular furnace, first at 500℃ for 5h, then at 700℃ for 14h, and finally cooled to room temperature with the furnace, ground and sieved to obtain zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material. (Zinc nitrate-1)

[0070] Comparative Example 9:

[0071] Weigh 3.72g Ni 0.90 Co 0.05 Mn 0.05 (OH)2, 0.25g Zn(NO3)2·6H2O and 1.74g LiOH·H2O powder and 0.4g PVP were added to 20mL ethanol, wherein nLi:n(Ni+Co+Mn+Zn)=1.05:1 (molar ratio), heated in a water bath at 80℃ and stirred for 2h, then dried in vacuum at 80℃, and sintered in sections in an oxygen-permeable tubular furnace, first at 500℃ for 5h, then at 700℃ for 14h, and finally cooled to room temperature with the furnace, ground and sieved to obtain zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material. (Zinc nitrate-2)

[0072] Comparative Example 10:

[0073] Weigh 3.60g Ni 0.90 Co 0.05 Mn 0.05 (OH)2, 0.61g Zn(NO3)2·6H2O and 1.73g LiOH·H2O powder and 0.4g PVP were added to 20mL ethanol, wherein nLi:n(Ni+Co+Mn+Zn)=1.05:1 (molar ratio), heated in a water bath at 80℃ and stirred for 2h, then vacuum dried at 80℃, and placed in an oxygen-permeable tubular furnace for staged sintering, first at 500℃ for 5h, then at 700℃ for 14h, and finally cooled to room temperature with the furnace, ground and sieved to obtain zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material. (Zinc nitrate-5)

[0074] Figure 1The XRD spectra of the positive electrode materials doped with zinc before and after zinc doping were compared. Comparative Examples 1-10 all showed typical structural characteristics of LiNiO2 positive electrode materials, and their diffraction peaks were characteristic peaks of a-NaFeO2 layered structure, belonging to the hexagonal system, R-3m space group. The two pairs of diffraction peaks (006) / (012) and (018) / (110) of the positive electrode materials of Examples 1 to 3 were obviously split, forming a better layered structure. The diffraction peaks of the materials did not change significantly before and after doping, and there were no impurity peaks. The peak intensity ratio of (003) to (104) was similar to that of the layered positive electrode material LiNiO2. + / Ni 2+ The degree of mixing is related to the peak intensity ratio I (003) / I (104) The larger the value, the lower the degree of cation mixing. (003) / I (104) The smallest, which may be due to the particle breakage caused by ball milling, resulting in a serious degree of cation mixing. In Comparative Examples 5 to 10, zinc acetate and zinc nitrate were used as zinc sources, respectively, and PVP was complexed with zinc ions and then sintered in stages. The corresponding peak intensity ratio I (003) / I (104) It is higher than that of Comparative Examples 2 to 4, but the degree of lithium-nickel intermixing is still higher than that of Examples 1 to 3. This is because the method of introducing zinc element into the layered structure by ALD coating of the ternary precursor followed by solid phase sintering causes the least damage to the secondary particles compared with other preparation methods.

[0075] Figure 2 It shows that as the lithium-extraction process of the electrode material continues, the capacity of the positive electrode material changes significantly before and after zinc doping modification, both of which are better than comparative example 1, indicating that zinc doping can effectively improve the cycle stability of the material. Figure 2 and Figure 3 It can be seen that the positive electrode materials of Example 2 and Comparative Example 1 are both formed by agglomeration of primary particles to form secondary particles with a particle size of about 3 μm. Doping modification does not change the overall morphology of the positive electrode material. Figure 4 The uniformity of the spherical particles of elements Ni, Co, Mn, and Zn is shown, proving the effectiveness of the process.

[0076] Figure 5 It shows that as the lithium insertion and extraction process continues, after Example 2 is cycled 200 times at a rate of 1C, the discharge capacity is still 176.7 mAh g -1 , the discharge specific capacity is higher than that of comparative example 1 and embodiments 1 and 3, which indicates that zinc plays a role in stabilizing the layered structure and is more conducive to improving the cycle stability of the material.

[0077] The present invention and its embodiments are described schematically above, and the description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. Therefore, if a person skilled in the art is inspired by it and designs a structural method and an embodiment similar to the technical solution without creativity without departing from the purpose of the invention, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material, characterized in that: Using Zn salt and water as raw materials, ZnO is coated on the surface of the nickel-cobalt-manganese ternary precursor through ALD, and then mixed with lithium salt and calcined at high temperature to finally obtain a Zn-doped ultra-high nickel ternary lithium-ion battery positive electrode material.

2. The method for preparing the zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material according to claim 1, characterized in that: The following steps are involved: Step 1, placing the dried nickel-cobalt-manganese ternary precursor powder on the ALD sample tray, using 10-25°C H2O as the oxidant of the Zn source, and selecting high-purity argon as the carrier gas and process purge gas, the temperature of the reaction outer chamber is set to 210°C, and the temperature of the inner chamber is set to 200°C. During deposition, first, the Zn source pulse is 150ms, wait for 10s, purge argon for 10s, wait for 5s, then pulse H2O for 100ms, wait for 5s, purge argon for 10s, and finally wait for 5s to enter the next cycle; after the set number of cycles, a ternary precursor with surface deposited ZnO is obtained; Step 2: Take the deposited ZnO ternary precursor and mix it evenly with LiOH·H2O, and calcine it in stages in a tubular atmosphere furnace with flowing oxygen, first keep it at 450-550°C for 4-6 hours, then keep it at 600-800°C for 12-16 hours, and finally cool it to room temperature with the furnace, grind and sieve to obtain zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material.

3. The method for preparing the zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material according to claim 2, characterized in that: The chemical formula of the ultra-high nickel ternary precursor is Ni 0.90 Co 0.05 Mn 0.05 (OH)2, the zinc source is diethyl zinc, and the lithium source is at least one of lithium nitrate, lithium acetate, lithium carbonate and lithium hydroxide.

4. The method for preparing the zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material according to claim 2, characterized in that: The vacuum drying temperature of the nickel-cobalt-manganese ternary precursor powder is 60-100°C.

5. The method for preparing the zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material according to claim 2, characterized in that: The mass of the dried nickel-cobalt-manganese ternary precursor powder placed on the ALD sample tray is 2g-4g.

6. The method for preparing the zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material according to claim 2, characterized in that: The number of ALD cycles is 25-200 times.

7. The method for preparing the zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material according to claim 3, characterized in that: Ni of the dried nickel-cobalt-manganese ternary precursor powder 0.90 Co 0.05 Mn 0.05 The mass ratio of (OH)2 to LiOH·H2O is 0.95:0.

46.

8. The method for preparing a zinc-doped ternary material precursor according to claim 2, characterized in that: After grinding in step 2, the mixture is sieved with a mesh size of 300.

9. The zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material prepared by the preparation method according to claim 1, characterized in that: The zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material has Ni≥0.9 mol, and its diffraction peak is a characteristic peak of a-NaFeO2 layered structure, belonging to the hexagonal crystal system and R-3m space group.

10. Use of the zinc-doped ultra-high nickel ternary lithium-ion battery positive electrode material prepared by the preparation method according to claim 1 as a positive electrode in a lithium-ion battery.

Citation Information

Patent Citations

  • Preparation method of modified lithium battery positive electrode material, modified lithium battery positive electrode material and lithium battery positive electrode structure

    CN114715946A

  • Positive electrode material and preparation method thereof, positive electrode plate, lithium ion battery and electric equipment

    CN117954608A

  • Cathode active material, manufacturing method thereof, and lithium secondary battery including same

    KR1020140073048A

Cited By

  • PVD (Physical Vapor Deposition) modified positive electrode material as well as preparation method and application thereof