Single crystal type layered oxide sodium ion battery positive electrode material and preparation method thereof

Through the combination of sodium source, nickel-ferromanganese ternary precursor and organic amine template agent, the problems of poor cycle stability and low energy density of the positive electrode material of single crystal transition metal layered oxide sodium ion battery are solved, and A single crystal layered sodium oxide positive electrode material with high energy density and good cycle stability has the potential for commercial application.

CN118908304APending Publication Date: 2024-11-08GEM WUXI ENERGY MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410982556.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing single-crystal transition metal layered sodium oxide battery positive electrode materials have poor cyclic stability and low energy density, which limits its promotion in energy storage and power application scenarios.

Method used

The complex precursor material is formed by solvent heat treatment using sodium source, nickel-ferromanganese ternary precursor, organic amine template agent, and solvent. After roasting and grinding, crystal nuclei are obtained, and then combined with nickel-ferromanganese ternary precursor and sodium source Mixed well and sintered, and high-temperature solid phase synthesis was performed by stepping sodium supplementation method to obtain a single crystal layered oxide sodium electropositive electrode material with high spherical shape, small specific surface area and high compaction density.

Benefits of technology

实现了高能量密度和较好循环稳定性,具有良好的商业化前景。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908304A_ABST
    Figure CN118908304A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sodium ion battery positive electrode materials, in particular to a single crystal type layered oxide sodium ion battery positive electrode material and a preparation method thereof. The preparation method of the single crystal type layered oxide sodium ion battery positive electrode material comprises the following steps: uniformly mixing a sodium source, a nickel-iron-manganese ternary precursor, an organic amine template agent and a solvent, and carrying out solvent heat treatment to obtain a complex precursor material; carrying out roasting treatment and grinding treatment on the complex precursor material to obtain a crystal nucleus; uniformly mixing the nickel-iron-manganese ternary precursor, a sodium source and a crystal nucleus to obtain blended powder, and sintering the blended powder to obtain the single crystal type layered oxide sodium ion battery positive electrode material. According to the invention, organic amines are adopted as a structure template agent, a solvothermal method is adopted to preliminarily form a crystal nucleus, and then a gradual sodium supplementing method is adopted to carry out high-temperature solid-phase synthesis to obtain the sodium battery positive electrode material, so that the sodium battery positive electrode material has high energy density and relatively good cycling stability in the aspect of electrochemical performance, and has a good commercial prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion battery positive electrode materials, and in particular to a single crystal layered oxide sodium ion battery positive electrode material and a preparation method thereof. Background Art

[0002] Lead-acid batteries are facing elimination due to their unavoidable environmental pollution. Among secondary batteries, lithium-ion batteries have the best performance, but the reserves of lithium resources are limited and there is a risk of exhaustion, which limits the development of lithium-ion batteries. Compared with lithium resources, the abundance of sodium resources is a major advantage of sodium-ion batteries. The working principle of sodium-ion batteries is similar to that of lithium-ion batteries, with lower costs and performance close to that of lithium batteries. To a certain extent, sodium-ion batteries can alleviate the problem of limited development of energy storage batteries caused by the shortage of lithium resources, and are an excellent alternative to lithium-ion batteries.

[0003] At present, the positive electrode materials used in sodium-ion batteries mainly include transition metal layered oxide systems (single crystal, polycrystalline), polyanion compounds (phosphate system, fluorophosphate system, NASICON structure) and Prussian blue system. Among them, single crystal transition metal layered oxides have attracted widespread attention due to their advantages of high capacity, low cost, and suitability for commercial development. However, this type of material is easy to form flaky single crystals, which makes the specific surface area of ​​the material larger. As the number of charge and discharge cycles increases, its surface side reactions will also increase sharply, resulting in poor cycle stability. In addition, its compaction density is also relatively small, resulting in a relatively low energy density, which limits its promotion in energy storage and power application scenarios. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of poor cycle stability and low energy density of existing single-crystal transition metal layered oxide sodium-ion battery positive electrode materials, thereby providing a single-crystal layered oxide sodium-ion battery positive electrode material and a preparation method thereof that solves the above problems.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing a single crystal layered oxide sodium ion battery positive electrode material comprises: mixing a sodium source, a nickel-iron-manganese ternary precursor, an organic amine template agent, and a solvent and performing a solvent thermal treatment to obtain a complex precursor material;

[0007] The complex precursor material is subjected to calcination and grinding to obtain a crystal nucleus;

[0008] The nickel-iron-manganese ternary precursor, the sodium source and the crystal nucleus are mixed to obtain a blending powder, and then the blending powder is sintered to obtain a single crystal layered oxide sodium ion battery positive electrode material.

[0009] Preferably, the sodium source is sodium carbonate;

[0010] And / or, the nickel-iron-manganese ternary precursor is Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2;

[0011] And / or, the organic amine template is n-butylamine;

[0012] And / or, the solvent is water.

[0013] Preferably, the mass ratio of the sodium source, the nickel-iron-manganese ternary precursor, and the solvent is (3-4): (5-6): (5-10);

[0014] And / or, based on the mass of the nickel-iron-manganese ternary precursor being 100 g, the amount of the organic amine template agent used is 50-100 mL.

[0015] Preferably, the temperature of the solvent thermal treatment is 200-240°C;

[0016] And / or, the duration of the solvent thermal treatment is 24-48h;

[0017] And / or, the solvent heat treatment is further followed by natural cooling and drying.

[0018] Preferably, the calcination temperature is 850-950°C;

[0019] And / or, the calcination treatment lasts for 7-10 hours;

[0020] And / or, the atmosphere of the calcination treatment is oxygen;

[0021] And / or, the grinding process is performed to a material particle size D50≤0.1 μm.

[0022] Preferably, the mass ratio of the nickel-iron-manganese ternary precursor to the sodium source in the blended powder is (5-6): (3-4);

[0023] And / or, the amount of crystal nuclei added to the blended powder is 1-2wt% of the total mass of the nickel-iron-manganese ternary precursor and the sodium source.

[0024] Preferably, the sintering temperature is 900-1000°C;

[0025] And / or, the sintering treatment time is 8-12h;

[0026] And / or, the atmosphere of the sintering process is air.

[0027] Preferably, after the sintering treatment, the raw material is mixed with TiO2 and subjected to a secondary sintering treatment.

[0028] Preferably, the amount of TiO2 is 0.5-1.5wt% of the mass of the material obtained by sintering;

[0029] And / or, the temperature of the secondary sintering treatment is 600-800°C;

[0030] And / or, the duration of the secondary sintering treatment is 6-10 hours;

[0031] And / or, the atmosphere of the secondary sintering treatment is air.

[0032] The present invention also provides a single crystal layered oxide sodium ion battery positive electrode material, which is prepared by the above-mentioned single crystal layered oxide sodium ion battery positive electrode material preparation method.

[0033] The technical solution of the present invention has the following advantages:

[0034] A method for preparing a single crystal layered oxide sodium ion battery positive electrode material, comprising: mixing a sodium source, a nickel-iron-manganese ternary precursor, an organic amine template, and a solvent, and performing a solvent thermal treatment to obtain a complex precursor material; performing a roasting treatment and a grinding treatment on the complex precursor material to obtain a crystal nucleus; mixing the nickel-iron-manganese ternary precursor, a sodium source, and a crystal nucleus to obtain a blending powder, and then sintering the blending powder to obtain a single crystal layered oxide sodium ion battery positive electrode material. The present invention uses organic amines as a structural template and a solvent thermal method to preliminarily form a crystal nucleus, and then uses a gradual sodium supplementation method to perform high-temperature solid phase synthesis to obtain a single crystal layered oxide sodium positive electrode material with high sphericity, small specific surface area, and high compaction density. In terms of electrochemical performance, it has high energy density and good cycle stability, and has good commercial prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 This is a scanning electron microscope image of the single crystal layered oxide sodium ion battery positive electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0037] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0038] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0039] Example 1

[0040] This embodiment provides a method for preparing a single crystal layered oxide sodium ion battery positive electrode material, and the specific steps are as follows:

[0041] 1) Weigh the solid drugs Na2CO3 (60g), Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 (100.00 g) was added to a 500 mL polytetrafluoroethylene liner containing 100 mL of deionized water, and then n-butylamine (50 mL) was added and stirred evenly with a glass rod;

[0042] 2) After all the drugs are weighed, the polytetrafluoroethylene liner is encapsulated in a stainless steel sleeve and placed in a 240°C oven for reaction for 48 hours. After the reaction is completed, the reactor is taken out, cooled to room temperature, washed with deionized water, and filtered. After the product is dried in a 120°C oven, a complex precursor material is obtained;

[0043] 3) The complex precursor material obtained in step 2) was heated in a box furnace at 900°C and an O2 atmosphere (3 m 3 / h), sintered for 10h, obtained O3 type NFM grains, fully ground into fine powder (D50≤0.1μm), obtained NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 nucleus;

[0044] 4) 5.0 kg of precursor Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 and 3.0kg sodium carbonate, 0.08kg NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 The O2 nuclei were mixed in a high-speed mixer and then heated in a box furnace at 1000°C in an air atmosphere (5m 3 / h), sintering for 12h, and then crushing to obtain a sodium positive electrode material-fired material (NFM);

[0045] 5) Weigh 500g of the first calcined material (NFM) in step 4) and 5g of TiO2 into a high-speed mixer and mix them evenly. Then, heat the mixture in a box furnace at 700°C in air atmosphere (5m 3 / h), sintered for 6h for secondary sintering coating, after sintering, a single crystal layered oxide sodium ion battery positive electrode material is obtained. The microstructure of the single crystal layered oxide sodium ion battery positive electrode material prepared in this embodiment is shown in FIG. Figure 1 shown.

[0046] Example 2

[0047] This embodiment provides a method for preparing a single crystal layered oxide sodium ion battery positive electrode material, and the specific steps are as follows:

[0048] 1) Weigh the solid drugs Na2CO3 (60g), Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 (100.00 g) was added to a 500 mL polytetrafluoroethylene liner containing 100 mL of deionized water, and then n-butylamine (50 mL) was added and stirred evenly with a glass rod;

[0049] 2) After all the drugs are weighed, the polytetrafluoroethylene liner is encapsulated in a stainless steel sleeve and placed in a 240°C oven for reaction for 48 hours. After the reaction is completed, the reactor is taken out, cooled to room temperature, washed with deionized water, and filtered. After the product is dried in a 120°C oven, a complex precursor material is obtained;

[0050] 3) The complex precursor material obtained in step 2) was heated in a box furnace at 900°C and an O2 atmosphere (3 m 3 / h), sintered for 10h, obtained O3 type NFM grains, fully ground into fine powder (D50≤0.1μm), obtained NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 nucleus;

[0051] 4) 5.0 kg of precursor Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 and 3.0kg sodium carbonate, 0.08kg NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 The O2 nuclei were mixed in a high-speed mixer and then heated in a box furnace at 1000°C in an air atmosphere (5m 3 / h), sintered for 12h, and then crushed to obtain a single crystal layered oxide sodium ion battery positive electrode material.

[0052] Example 3

[0053] This embodiment provides a method for preparing a single crystal layered oxide sodium ion battery positive electrode material, and the specific steps are as follows:

[0054] 1) Weigh solid drugs Na2CO3 (50g), Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 (100.00 g) was added to a 500 mL polytetrafluoroethylene liner containing 150 mL deionized water, and then n-butylamine (50 mL) was added and stirred evenly with a glass rod;

[0055] 2) After all the drugs are weighed, the polytetrafluoroethylene liner is encapsulated in a stainless steel sleeve and placed in a 200°C oven for reaction for 24 hours. After the reaction is completed, the reactor is taken out, cooled to room temperature, washed with deionized water, and filtered. After the product is dried in an oven at 120°C, a complex precursor material is obtained;

[0056] 3) The complex precursor material obtained in step 2) was heated in a box furnace at 850°C and an O2 atmosphere (3m 3 / h), sintered for 7h, obtained O3 type NFM grains, fully ground into fine powder (D50≤0.1μm), obtained NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 nucleus;

[0057] 4) 6.0 kg of precursor Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 and 4.0kg sodium carbonate, 0.16kg NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 The O2 nuclei were mixed in a high-speed mixer and then heated in a box furnace at 900°C in an air atmosphere (5m 3 / h), sintering for 8h, and then crushing to obtain a sodium positive electrode material-fired material (NFM);

[0058] 5) Weigh 500 g of the first calcined material (NFM) in step 4) and 2.5 g of TiO2, add them into a high-speed mixer and mix them evenly. Then, heat them in a box furnace at 700°C and air atmosphere (5 m 3 / h), sintering for 6h for secondary sintering coating, and after the sintering is completed, a single crystal layered oxide sodium ion battery positive electrode material is obtained.

[0059] Example 4

[0060] This embodiment provides a method for preparing a single crystal layered oxide sodium ion battery positive electrode material, and the specific steps are as follows:

[0061] 1) Weigh the solid drugs Na2CO3 (80g), Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 (100.00 g) was added to a 500 mL polytetrafluoroethylene liner containing 200 mL of deionized water, and then n-butylamine (100 mL) was added and stirred evenly with a glass rod;

[0062] 2) After all the drugs are weighed, the polytetrafluoroethylene liner is encapsulated in a stainless steel sleeve and placed in a 240°C oven for reaction for 48 hours. After the reaction is completed, the reactor is taken out, cooled to room temperature, washed with deionized water, and filtered. After the product is dried in a 120°C oven, a complex precursor material is obtained;

[0063] 3) The complex precursor material obtained in step 2) was heated in a box furnace at 950°C and an O2 atmosphere (3m 3 / h), sintered for 10h, obtained O3 type NFM grains, fully ground into fine powder (D50≤0.1μm), obtained NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 nucleus;

[0064] 4) 5.0 kg of precursor Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 and 3.0kg sodium carbonate, 0.08kg NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 The O2 nuclei were mixed in a high-speed mixer and then heated in a box furnace at 1000°C in an air atmosphere (5m 3 / h), sintering for 12h, and then crushing to obtain a sodium positive electrode material-fired material (NFM);

[0065] 5) Weigh 500 g of the first calcined material (NFM) in step 4) and 7.5 g of TiO2 into a high-speed mixer and mix well. Then, heat in a box furnace at 700°C in air atmosphere (5 m 3 / h), sintering for 6h for secondary sintering coating, and after the sintering is completed, a single crystal layered oxide sodium ion battery positive electrode material is obtained.

[0066] Comparative Example 1

[0067] This comparative example provides a method for preparing a single-crystal layered oxide sodium ion battery positive electrode material, and the specific steps are as follows:

[0068] 1) 5.0 kg of precursor Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH)2 was mixed with 3.0 kg of sodium carbonate in a high-speed mixer and then heated in a box furnace at 1000 °C in an air atmosphere (5 m 3 / h), sintering for 12h, and then crushing to obtain a sodium positive electrode material-fired material (NFM);

[0069] 2) Weigh 500g of the first calcined material (NFM) in step 2) and 5g of TiO2 into a high-speed mixer and mix them evenly. Then, heat the mixture in a box furnace at 700°C and air atmosphere (5m 3 / h), sintering for 6h for secondary sintering coating, and after the sintering is completed, a single crystal layered oxide sodium ion battery positive electrode material is obtained.

[0070] Test Example 1

[0071] The positive electrode materials of the sodium ion battery of the embodiment and the comparative example were mixed with the conductive agent acetylene carbon black and the binder PVDF in a mass ratio of 95:2.5:2.5, respectively, and an appropriate amount of 1-methyl-2-pyrrolidone was added and ball-milled for 1 hour to make a slurry, which was evenly coated on the aluminum sheet, dried to remove the 1-methyl-2-pyrrolidone, and pressed into a positive electrode sheet. The negative electrode was a metal sodium sheet, and the electrolyte was sodium hexafluorophosphate (NaPF6) as the electrolyte, and a mixture of ethylene carbonate (EC) and dimethyl carbonate (DMC) with a volume ratio of 1:1 as the solvent. The electrolyte concentration in the electrolyte was 1 mol / L, and assembled into a 2032 button battery. The electrical performance test was performed using the Siken test system. The first cycle was charged and discharged at a rate of 0.1C within the cut-off voltage range of 2.0-4.5V, and then the cycle was cycled 50 times under the condition of a charge and discharge rate of 1C to test the cycle capacity retention rate. The test results are shown in Table 1.

[0072] Table 1

[0073]

[0074] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a single crystal layered oxide sodium ion battery positive electrode material, It is characterized in that include: A sodium source, a nickel-iron-manganese ternary precursor, an organic amine template, and a solvent are mixed and subjected to solvent thermal treatment to obtain a complex precursor material; The complex precursor material is subjected to calcination and grinding to obtain a crystal nucleus; The nickel-iron-manganese ternary precursor, the sodium source and the crystal nucleus are mixed to obtain a blending powder, and then the blending powder is sintered to obtain a single crystal layered oxide sodium ion battery positive electrode material.

2. The preparation method according to claim 1, It is characterized in that The sodium source is sodium carbonate; And / or, the nickel-iron-manganese ternary precursor is Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 (OH) 2 ; And / or, the organic amine template is n-butylamine; And / or, the solvent is water.

3. The preparation method according to claim 1 or 2, It is characterized in that The mass ratio of the sodium source, the nickel-iron-manganese ternary precursor, and the solvent is (3-4): (5-6): (5-10); And / or, based on the mass of the nickel-iron-manganese ternary precursor being 100 g, the amount of the organic amine template agent used is 50-100 mL.

4. The preparation method according to any one of claims 1 to 3, It is characterized in that The temperature of the solvent thermal treatment is 200-240°C; And / or, the duration of the solvent thermal treatment is 24-48h; And / or, the solvent heat treatment is further followed by natural cooling and drying.

5. The preparation method according to any one of claims 1 to 4, It is characterized in that The calcination temperature is 850-950°C; And / or, the calcination treatment lasts for 7-10 hours; And / or, the atmosphere of the calcination treatment is oxygen; And / or, the grinding process is performed to a material particle size D50≤0.1 μm.

6. The preparation method according to any one of claims 1 to 5, It is characterized in that The mass ratio of the nickel-iron-manganese ternary precursor to the sodium source in the blended powder is (5-6): (3-4); And / or, the amount of crystal nuclei added to the blended powder is 1-2wt% of the total mass of the nickel-iron-manganese ternary precursor and the sodium source.

7. The preparation method according to any one of claims 1 to 6, It is characterized in that The sintering temperature is 900-1000°C; And / or, the sintering treatment time is 8-12h; And / or, the atmosphere of the sintering process is air.

8. The preparation method according to any one of claims 1 to 7, It is characterized in that After the sintering treatment, TiO 2 Mix well and perform secondary sintering.

9. The preparation method according to claim 8, It is characterized in that The TiO 2 The dosage is 0.5-1.5wt% of the mass of the material obtained by sintering; And / or, the temperature of the secondary sintering treatment is 600-800°C; And / or, the duration of the secondary sintering treatment is 6-10 hours; And / or, the atmosphere of the secondary sintering treatment is air.

10. A single crystal layered oxide sodium ion battery positive electrode material, It is characterized in that The positive electrode material is prepared by the method for preparing the single-crystal layered oxide sodium ion battery positive electrode material according to any one of claims 1 to 9.

Citation Information

Cited By

  • Preparation method and application of sodium ion layered oxide cathode material nickel iron sodium manganate

    CN119637955A