Lead-free diode glass bulb and preparation method thereof
By controlling the surface roughness and sandblasting process in the lead-free diode glass shell, the problems of high sealing temperature and poor heat resistance are solved, and low sealing temperature and high heat resistance are achieved, avoiding environmental hazards and simplifying recycling deal with.
Patent Information
- Application Number
- CN202411009483.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lead-free glass crust has a high sealing temperature and poor thermal impact resistance to small-sized chips, making it difficult to match, and the lead-containing glass crust is complex to recover and handle, which has environmental hazards.
45-55% SiO2, 10-20% B2O3, 10-22% alkali metal oxide, 0.8-8% alkaline earth metal oxide, 0.5-4% Al2O3, 5-12% TiO2, 0.5 were used. -4% ZnO, 0.1-4% clarifier-free diode glass shell, through the control of the surface roughness and sandblasting process of glass shell, surfaces with different roughness are formed, reducing the sealing temperature and improving heat resistance.
It achieves a low sealing temperature, improves the service life and heat resistance of the product, avoids environmental hazards of lead elements, and simplifies recycling and processing.
Smart Images

Figure BDA0004963901810000081 
Figure BDA0004963901810000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass manufacturing, in particular to a lead-free diode glass shell and a preparation method thereof. Background Art
[0002] Small diodes, such as silicon diodes, light-emitting diodes and thermistors, are usually packaged in leaded glass shells, that is, the diode chip is sandwiched between a pair of electrodes, and the external lead wire and the leaded glass shell are softened and sealed together by heating to form an airtight structure. The lead element in the leaded glass shell is harmful to both the human body and the environment, and when recycling equipment containing leaded glass shells, the glass shell needs to be removed from the equipment and handled separately.
[0003] In order to avoid the above adverse effects, in the related technology, lead-free glass shells made of lead-free glass are used in the packaging of diodes, but the sealing temperature of such lead-free glass shells is relatively high, and the chip will be damaged when heated and sealed with magnesium wire. And now as the size of chips is reduced and the internal structure is becoming more and more sophisticated, a lead-free packaging glass shell that can match the poor thermal shock resistance of small-sized chips is needed. Summary of the invention
[0004] The object of the present invention is to provide a lead-free diode glass shell and a preparation method thereof to solve the problems raised in the above background technology.
[0005] According to a first aspect of the present invention, a lead-free diode glass shell is provided, which mainly comprises the following raw materials in weight percentage: 45-55% SiO2; 10-20% B2O3; 10-22% alkali metal oxide; 0.8-8% alkaline earth metal oxide; 0.5-4% Al2O3; 5-12% TiO2; 0.5-4% ZnO; 0.1-4% clarifier; wherein the alkali metal oxide comprises one or more combinations of Li2O, Na2O and K2O; the alkaline earth metal oxide comprises one or more combinations of MgO, CaO, SrO and BaO; the lead-free diode glass shell comprises two large faces arranged opposite to each other, wherein the roughness Ra of one face is a, and the roughness Ra of the other face is b, 0.8≤a / b≤1.2; the large face is the face with the largest surface area in the lead-free diode glass shell.
[0006] The present invention controls the roughness of two surfaces of the glass shell when preparing the lead-free diode glass shell, so that the glass shell surface has different refractive indices for the pipeline, ensuring the glass shell's ability to absorb laser light. At the same time, since the roughness on the two surfaces of the glass shell is inconsistent, the excessive expansion of the glass shell after post-heating can be prevented, ensuring the service life of the product. At the same time, since the glass shell surface has a certain roughness, the sealing temperature can be reduced during sealing, thereby improving the service life of the product.
[0007] In a second aspect, the present invention provides a method for preparing a lead-free diode glass shell, comprising the following steps:
[0008] (1) Weigh 45-55% SiO2, 10-20% B2O3, 10-22% alkali metal oxide, 0.8-8% alkaline earth metal oxide, 0.5-4% Al2O3, 5-12% TiO2, 0.5-4% ZnO, and 0-4% clarifier in order by weight percentage;
[0009] (2) mixing the raw materials weighed in step (1) to obtain a mixture, and feeding the obtained mixture into an electric melting furnace to melt it at a temperature of 1200 to 1300° C. to form molten glass;
[0010] (3) the glass liquid obtained in step (2) is clarified and homogenized at 1100-1200° C. for 20-30 min, and then drawn into a tube at 700-900° C. to obtain a glass bulb blank;
[0011] (4) The glass shell blank obtained in step (3) is sandblasted by a sandblasting machine and then cut to obtain a lead-free diode glass shell.
[0012] When preparing the lead-free diode glass bulb, the present invention controls the borax rate of the sandblasting process on different surfaces of the glass bulb so that two surfaces of the glass bulb have different roughnesses, thereby making the glass bulb have good heat resistance and laser absorption ability during use. DETAILED DESCRIPTION
[0013] According to a first aspect of the present invention, a lead-free diode glass shell is provided, which mainly comprises the following raw materials in weight percentage: 45-55% SiO2; 10-20% B2O3; 10-22% alkali metal oxide; 0.8-8% alkaline earth metal oxide; 0.5-4% Al2O3; 5-12% TiO2; 0.5-4% ZnO; 0.1-4% clarifier; wherein the alkali metal oxide comprises one or more combinations of Li2O, Na2O and K2O; the alkaline earth metal oxide comprises one or more combinations of MgO, CaO, SrO and BaO; the lead-free diode glass shell comprises two large faces arranged opposite to each other, wherein the roughness Ra of one face is a, and the roughness Ra of the other face is b, 0.8≤a / b≤1.2; the large face is the face with the largest surface area in the lead-free diode glass shell.
[0014] Preferably, the weight percentage mixing ratio of Li2O, Na2O and K2O in the alkali metal oxide is 1:(1-1.3):(0.5-1.2).
[0015] Preferably, the weight percentage of Li2O is 3-8%.
[0016] Preferably, the clarifier includes one or a combination of Sb2O3 and CeO2.
[0017] Preferably, the range of a is 7 to 12 μm, and the range of b is 8.5 to 24 μm.
[0018] In a second aspect, the present invention provides a method for preparing a lead-free diode glass shell, comprising the following steps:
[0019] (1) Weigh 45-55% SiO2, 10-20% B2O3, 10-22% alkali metal oxide, 0.8-8% alkaline earth metal oxide, 0.5-4% Al2O3, 5-12% TiO2, 0.5-4% ZnO, and 0-4% clarifier in order by weight percentage;
[0020] (2) mixing the raw materials weighed in step (1) to obtain a mixture, and feeding the obtained mixture into an electric melting furnace to melt it at a temperature of 1200 to 1300° C. to form molten glass;
[0021] (3) the glass liquid obtained in step (2) is clarified and homogenized at 1100-1200° C. for 20-30 min, and then drawn into a tube at 700-900° C. to obtain a glass bulb blank;
[0022] (4) The glass shell blank obtained in step (3) is sandblasted by a sandblasting machine and then cut to obtain a lead-free diode glass shell.
[0023] Preferably, the sand used for the sandblasting in step (4) is one of silicon dioxide or silicon carbide, and the particle size of the sand is 80 to 120 microns.
[0024] Preferably, the sandblasting process conditions in step (4) are as follows: the average sandblasting rate on one large surface of the glass shell is 50 m / s to 80 m / s, and the sandblasting time is 50 to 100 s; the average sandblasting rate on the other large surface of the glass shell is 30 to 45 m / s, and the sandblasting time is 10 to 30 s.
[0025] Example 1
[0026] A lead-free diode glass shell, measured by weight percentage, mainly comprises:
[0027] 45% SiO2; 10% B2O3; 10% Na2O; 0.8% MgO; 0.5% Al2O3; 5% TiO2; 0.5% ZnO; 0.1% Sb2O3.
[0028] A method for preparing a lead-free diode glass shell comprises the following steps:
[0029] (1) Weigh 45% SiO2, 10% B2O3, 10% Na2O, 0.8% MgO, 0.5% Al2O3, 5% TiO2, 0.5% ZnO, and 0.1% Sb2O3 in order by weight;
[0030] (2) mixing the raw materials weighed in step (1) to obtain a mixture, and feeding the obtained mixture into an electric melting furnace to melt it at a temperature of 1200° C. to form molten glass;
[0031] (3) the glass liquid obtained in step (2) is clarified and homogenized at 1100° C. for 20 min, and then drawn into a tube at 700° C. to obtain a glass bulb blank;
[0032] (4) The glass shell blank obtained in step (3) is sandblasted by a sandblasting machine and then cut to obtain a lead-free diode glass shell.
[0033] Preferably, the sand used in the sandblasting in step (4) is silicon dioxide, and the particle size of the silicon dioxide is 80 microns.
[0034] Preferably, the sandblasting process conditions in step (4) are as follows: the average sandblasting rate on one large surface of the glass shell is 75 m / s, and the sandblasting time is 60 s; the average sandblasting rate on the other large surface of the glass shell is 30 m / s, and the sandblasting time is 10 s.
[0035] Example 2
[0036] A lead-free diode glass shell, measured by weight percentage, mainly comprises:
[0037] 55% SiO2; 20% B2O3; 22% Na2O; 8% MgO; 4% Al2O3; 12% TiO2; 4% ZnO; 4% Sb2O3.
[0038] A method for preparing a lead-free diode glass shell comprises the following steps:
[0039] (1) Weigh 55% SiO2, 20% B2O3, 22% Na2O, 8% MgO, 4% Al2O3, 12% TiO2, 4% ZnO, and 4% Sb2O3 in order by weight;
[0040] (2) mixing the raw materials weighed in step (1) to obtain a mixture, and feeding the obtained mixture into an electric melting furnace to melt it at a temperature of 1300° C. to form molten glass;
[0041] (3) the glass liquid obtained in step (2) is clarified and homogenized at 1200° C. for 30 min, and then drawn into a tube at 900° C. to obtain a glass shell blank;
[0042] (4) The glass shell blank obtained in step (3) is sandblasted by a sandblasting machine and then cut to obtain a lead-free diode glass shell.
[0043] Preferably, the sand used in the sandblasting in step (4) is silicon dioxide, and the particle size of the silicon dioxide is 120 microns.
[0044] Preferably, the sandblasting process conditions in step (4) are as follows: the average sandblasting rate on one large surface of the glass shell is 60 m / s, and the sandblasting time is 100 s; the average sandblasting rate on the other large surface of the glass shell is 45 m / s, and the sandblasting time is 30 s.
[0045] Example 3
[0046] A lead-free diode glass shell, measured by weight percentage, mainly comprises:
[0047] 50% SiO2; 15% B2O3; 16% Na2O; 4% MgO; 2% Al2O3; 10% TiO2; 2% ZnO; 2% Sb2O3.
[0048] A method for preparing a lead-free diode glass shell comprises the following steps:
[0049] (1) Weigh 50% SiO2, 15% B2O3, 16% Na2O, 4% MgO, 2% Al2O3, 10% TiO2, 2% ZnO, and 2% Sb2O3 in order by weight;
[0050] (2) mixing the raw materials weighed in step (1) to obtain a mixture, and feeding the obtained mixture into an electric melting furnace to melt it at a temperature of 1250° C. to form molten glass;
[0051] (3) the glass liquid obtained in step (2) is clarified and homogenized at 1150° C. for 25 min, and then drawn into a tube at 800° C. to obtain a glass bulb blank;
[0052] (4) The glass shell blank obtained in step (3) is sandblasted by a sandblasting machine and then cut to obtain a lead-free diode glass shell.
[0053] Preferably, the sand used in the sandblasting in step (4) is silicon dioxide, and the particle size of the silicon dioxide is 80 microns.
[0054] Preferably, the sandblasting process conditions in step (4) are as follows: the average sandblasting rate on one large surface of the glass shell is 70 m / s, and the sandblasting time is 95 s; the average sandblasting rate on the other large surface of the glass shell is 30 m / s, and the sandblasting time is 20 s.
[0055] Comparative Example 1
[0056] A lead-free diode glass shell, measured by weight percentage, mainly comprises:
[0057] 44% SiO2; 9% B2O3; 9% Na2O; 0.7% MgO; 0.4% Al2O3; 4.8% TiO2; 0.4% ZnO; 0.08% Sb2O3.
[0058] A method for preparing a lead-free diode glass shell comprises the following steps:
[0059] (1) Weigh 44% SiO2, 9% B2O3, 9% Na2O, 0.7% MgO, 0.4% Al2O3, 4.8% TiO2, 0.4% ZnO, and 0.08% Sb2O3 in order by weight;
[0060] (2) mixing the raw materials weighed in step (1) to obtain a mixture, and feeding the obtained mixture into an electric melting furnace to melt it at a temperature of 1200° C. to form molten glass;
[0061] (3) the glass liquid obtained in step (2) is clarified and homogenized at 1100° C. for 20 min, and then drawn into a tube at 700° C. to obtain a glass bulb blank;
[0062] (4) The glass shell blank obtained in step (3) is sandblasted by a sandblasting machine and then cut to obtain a lead-free diode glass shell.
[0063] Preferably, the sand used in the sandblasting in step (4) is silicon dioxide, and the particle size of the silicon dioxide is 80 microns.
[0064] Preferably, the sandblasting process conditions in step (4) are as follows: the average sandblasting rate on one large surface of the glass shell is 80 m / s, and the sandblasting time is 80 s; the average sandblasting rate on the other large surface of the glass shell is 29 m / s, and the sandblasting time is 9 s.
[0065] Comparative Example 2
[0066] A lead-free diode glass shell, measured by weight percentage, mainly comprises:
[0067] 56% SiO2; 21% B2O3; 23% Na2O; 9% MgO; 5% Al2O3; 13% TiO2; 5% ZnO; 5% Sb2O3.
[0068] A method for preparing a lead-free diode glass shell comprises the following steps:
[0069] (1) Weigh 56% SiO2, 21% B2O3, 23% Na2O, 9% MgO, 5% Al2O3, 13% TiO2, 5% ZnO, and 5% Sb2O3 in order by weight;
[0070] (2) mixing the raw materials weighed in step (1) to obtain a mixture, and feeding the obtained mixture into an electric melting furnace to melt it at a temperature of 1300° C. to form molten glass;
[0071] (3) the glass liquid obtained in step (2) is clarified and homogenized at 1200° C. for 30 min, and then drawn into a tube at 900° C. to obtain a glass shell blank;
[0072] (4) The glass shell blank obtained in step (3) is sandblasted by a sandblasting machine and then cut to obtain a lead-free diode glass shell.
[0073] Preferably, the sand used in the sandblasting in step (4) is silicon dioxide, and the particle size of the silicon dioxide is 120 microns.
[0074] Preferably, the sandblasting process conditions in step (4) are as follows: the average sandblasting rate on one large surface of the glass shell is 60 m / s, and the sandblasting time is 70 s; the average sandblasting rate on the other large surface of the glass shell is 45 m / s, and the sandblasting time is 30 s.
[0075] Test Case
[0076] (1) Thermal expansion coefficient and heat sealing temperature
[0077] The linear expansion coefficient of the glass rod of the lead-free diode glass shell obtained in Examples 1 to 3 and Comparative Examples 1 to 2 was measured at 30-300° C. according to the ATSMD696 standard. The specific results are shown in Table 1.
[0078] The lead-free diode glass shells obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were measured for the sealing temperature of the glass fibers according to the ASTM C338 standard.
[0079] (2) Refractive index test
[0080] The refractive index of the lead-free diode glass shells obtained in Examples 1 to 3 and Comparative Examples 1 to 2 was tested according to the standard GB / T 7962.
[0081] (3) Roughness test
[0082] The roughness of the two large surfaces of the lead-free diode glass shells obtained in Examples 1 to 3 and Comparative Examples 1 to 2 was measured by a contact method according to standard ISO 25178, and the values were recorded, with the smaller value being recorded as a and the larger value being recorded as b, and the value of a / b was calculated.
[0083] Table 1 shows the test results of the lead-free diode glass shell performance obtained in Examples 1 to 3 and Comparative Examples 1 to 2
[0084]
[0085]
[0086] The lead-free diode glass shells obtained by Examples 1 to 3 and Comparative Examples 1 to 2 in Table 1 have a lower heat-sealing temperature, a large refractive index, and a small thermal expansion coefficient.
[0087] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A lead-free diode glass shell, characterized in that: The lead-free diode glass shell contains the following components in weight percentage: 45-55% SiO2; 10-20% B2O3; 10-22% alkali metal oxide; 0.8-8% alkaline earth metal oxide; 0.5-4% Al2O3; 5-12% TiO2; 0.5-4% ZnO; 0.1-4% clarifier; The alkali metal oxide includes one or more combinations of Li2O, Na2O and K2O; the alkaline earth metal oxide includes one or more combinations of MgO, CaO, SrO and BaO; the lead-free diode glass shell includes two large surfaces arranged opposite to each other, one of which has a roughness Ra of a and the other has a roughness Ra of b, 0.5≤a / b≤0.8; the large surface is the surface with the largest surface area in the lead-free diode glass shell.
2. The lead-free diode glass shell according to claim 1, characterized in that: The weight percentage mixing ratio of Li2O, Na2O and K2O in the alkali metal oxide is 1:(1-1.3):(0.5-1.2).
3. The lead-free diode glass shell according to claim 2, characterized in that: The weight percentage of Li2O is 3-8%.
4. The lead-free diode glass shell according to claim 1, characterized in that: The fining agent includes one or a combination of Sb2O3 and CeO2.
5. The lead-free diode glass shell according to claim 1, characterized in that: The range of a is 7 to 12 μm, and the range of b is 8.5 to 24 μm.
6. A method for preparing a lead-free diode glass shell, characterized in that: The following steps are involved: (1) Weigh 45-55% SiO2, 10-20% B2O3, 10-22% alkali metal oxide, 0.8-8% alkaline earth metal oxide, 0.5-4% Al2O3, 5-12% TiO2, 0.5-4% ZnO, and 0-4% clarifier in order by weight percentage; (2) mixing the raw materials weighed in step (1) to obtain a mixture, and feeding the obtained mixture into an electric melting furnace to melt it at a temperature of 1200 to 1300° C. to form molten glass; (3) the glass liquid obtained in step (2) is clarified and homogenized at 1100-1200° C. for 20-30 min, and then drawn into a tube at 700-900° C. to obtain a glass bulb blank; (4) The glass shell blank obtained in step (3) is sandblasted by a sandblasting machine and then cut to obtain a lead-free diode glass shell.
7. The method for preparing a lead-free diode glass shell according to claim 6, characterized in that: The sand used in the sandblasting process in step (4) is one of silicon dioxide and silicon carbide, and the particle size of the sand is 80 to 120 microns.
8. The method for preparing a lead-free diode glass shell according to claim 6, characterized in that: The sandblasting process conditions of step (4) are as follows: the average sandblasting rate on one large surface of the glass shell is 50m / s-80m / s, and the sandblasting time is 50-100s; the average sandblasting rate on the other large surface of the glass shell is 30-45m / s, and the sandblasting time is 10-30s.
Citation Information
Patent Citations
Lead-free low-temperature glass for manufacturing diode glass shell
CN102633435A
Local structure's glass cover plate's photovoltaic module with improvement mist degree has
CN208368519U