High-refraction high-dispersion optical glass
By reasonably adjusting the component ratio of oxides such as P2O5, Nb2O5, TiO2 in optical glass, the problem of large thermal expansion coefficient of optical glass in temperature changes is solved, and the combination of high refractive index and low thermal expansion coefficient is achieved, which is suitable for high Stable optical elements.
Patent Information
- Application Number
- CN202411158155.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
AI Technical Summary
The existing optical glass has a large thermal expansion coefficient in an environment with large temperature changes, which leads to changes in the imaging characteristics of the optical components and is difficult to meet the needs of high refractive index and low thermal expansion coefficient.
High refractive and high dispersion optical glass composed of oxides such as P2O5, Nb2O5, TiO2 and Na2O are used to optimize the refractive index, dispersion and thermal expansion coefficient of the glass by reasonably adjusting the component ratio, controlling the ratio of P2O5/Nb2O5, TiO2/Nb2O5 and other ratios.
It realizes optical glass with a low thermal expansion coefficient while having a high refractive index and high dispersion. It is suitable for environments with large temperature changes and improves the stability and imaging characteristics of optical components.
Smart Images

Figure BDA0005005662610000161 
Figure BDA0005005662610000171 
Figure BDA0005005662610000172
Abstract
Description
Technical Field
[0001] The invention relates to an optical glass, in particular to a high-refractive and high-dispersion optical glass with a low thermal expansion coefficient. Background Art
[0002] As people's living standards continue to improve, people's lives are becoming more and more colorful, and electronic devices such as wearable devices are also developing rapidly with the times. As wearable devices such as glasses with projectors, glasses-type or goggle-type displays, virtual reality augmented reality display devices, virtual image display devices, etc., the glass used is required to have a high refractive index from the perspectives of wide-angle images, high brightness, improved light-guiding properties, and ease of processing of diffraction gratings. In addition, in the past, small-sized shooting glass lenses with a wide shooting angle of view were used in applications such as vehicle-mounted cameras and robot visual sensors. For such shooting glass lenses, a high refractive index is required in order to be smaller and shoot a wider range.
[0003] With the popularity of surveillance security and vehicle-mounted imaging, the demand for optical components mounted on these devices continues to increase. High refractive index optical glass is an optical material that can be widely used in these fields. Optical components installed in vehicle-mounted equipment or instruments, as well as optical components installed in heat-generating optical instruments such as projectors, copiers, and laser printers, are used in environments with large temperature changes. If the thermal expansion coefficient of the optical glass is too large, the thermal expansion of the optical component will occur due to changes in ambient temperature. Because the expansion coefficient is different from that of the optical component fixing fixture, stress is generated in the optical component, which in turn generates birefringence, causing changes in imaging characteristics. Therefore, it is expected that optical glass has a lower thermal expansion coefficient. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a high-refractive and high-dispersion optical glass with a low thermal expansion coefficient.
[0005] The technical solution adopted by the present invention to solve the technical problem is:
[0006] (1) High refractive and high dispersion optical glass, the components of which are expressed in weight percentage and contain: 2 O 5 :20~34%;Nb 2 O 5 :38~53%;TiO 2 :8~22%;Na 2 O: 1-12%, of which P 2 O 5 / Nb 2 O 5 It is 0.4~0.85.
[0007] (2) The high-refractive and high-dispersion optical glass according to (1), wherein the components, expressed in weight percentage, further contain: BaO: 0-8%; and / or K 2 O: 0-10%; and / or CaO: 0-8%; and / or MgO: 0-5%; and / or SrO: 0-5%; and / or Li 2 O: 0-6%; and / or SiO 2 :0~5%;and / or B 2 O 3 :0~5%;and / or ZrO 2 : 0-5%; and / or Al 2 O 3 : 0-5%; and / or ZnO: 0-5%; and / or WO 3 :0~5%;and / or Ln 2 O 3 :0~5%; and / or Bi 2 O 3 : 0-5%; and / or clarifier: 0-1%, the Ln 2 O 3 For La 2 O 3 , Gd 2 O 3 , Y 2 O 3 , Yb 2 O 3 One or more of the following, the clarifier is Sb 2 O 3 SnO 2 , SnO, CeO 2 One or more of .
[0008] (3) High refractive and high dispersion optical glass, whose components contain P 2 O 5 , Nb 2 O 5 、TiO 2 and Na 2 O, whose components are expressed in weight percentage, where P 2 O 5 / Nb 2 O 5 The refractive index n of the high-refractive and high-dispersion optical glass is 0.4 to 0.85. d is 1.895~1.95, Abbe number ν d The thermal expansion coefficient is 15 to 22. 100 / 300℃ 100×10 -7 / K or less.
[0009] (4) The high-refractive and high-dispersion optical glass according to (3), wherein the components thereof are expressed in weight percentage and contain: 2 O 5 :20~34%;and / or Nb 2 O 5 :38~53%;and / or TiO 2 :8~22%;and / or Na 2 O: 1-12%; and / or K 2 O: 0-10%; and / or BaO: 0-8%; and / or CaO: 0-8%; and / or MgO: 0-5%; and / or SrO: 0-5%; and / or Li 2 O: 0-6%; and / or SiO 2 :0~5%;and / or B 2 O 3 :0~5%;and / or ZrO 2 : 0-5%; and / or Al 2 O 3 : 0-5%; and / or ZnO: 0-5%; and / or WO 3 :0~5%;and / or Ln 2 O 3 :0~5%; and / or Bi 2 O 3 : 0-5%; and / or clarifier: 0-1%, the Ln 2 O 3 For La 2 O 3 , Gd 2 O 3 , Y 2 O 3 , Yb 2 O 3 One or more of the following, the clarifier is Sb 2 O 3 SnO 2 , SnO, CeO 2 One or more of .
[0010] (5) The high-refractive and high-dispersion optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: (Nb 2 O 5 +Na 2 O+BaO) / TiO 2 is 1.8 to 5.5, preferably (Nb 2 O 5 +Na 2 O+BaO) / TiO 2 is 2.0 to 5.0, more preferably (Nb 2 O5 +Na 2 O+BaO) / TiO 2 2.5 to 4.5; and / or P 2 O 5 / Nb 2 O 5 0.45~0.8, preferably P 2 O 5 / Nb 2 O 5 0.5 to 0.7, more preferably P 2 O 5 / Nb 2 O 5 0.55 to 0.65; and / or TiO 2 / Nb 2 O 5 0.2 to 0.55, preferably TiO 2 / Nb 2 O 5 0.2 to 0.5, more preferably TiO 2 / Nb 2 O 5 0.25 to 0.45; and / or TiO 2 / K 2 O is 1.0 to 18.0, preferably TiO 2 / K 2 O is 1.0 to 12.0, more preferably TiO 2 / K 2 O is 1.5 to 10.0, and more preferably TiO 2 / K 2 O is 2.0 to 8.0; and / or (TiO 2 +K 2 O) / (BaO+Na 2 O) is 1.6 to 12.0, preferably (TiO 2 +K 2 O) / (BaO+Na 2 O) is 2.0 to 10.0, and more preferably (TiO 2 +K 2 O) / (BaO+Na 2 O) is 2.2 to 7.0, and more preferably (TiO 2 +K 2 O) / (BaO+Na 2 O) is 2.5 to 5.5; and / or CaO / BaO is 0.1 to 10.0, preferably CaO / BaO is 0.2 to 7.0, more preferably CaO / BaO is 0.3 to 5.0, and further preferably CaO / BaO is 0.5 to 3.0.
[0011] (6) The high-refractive and high-dispersion optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: 2 O 3 +SiO 2 ) / CaO is 2.8 or less, preferably (B 2 O 3 +SiO 2 ) / CaO is 0.1 to 2.0, more preferably (B 2 O 3 +SiO 2 ) / CaO is 0.2 to 1.5, and more preferably (B 2 O 3 +SiO 2 ) / CaO is 0.4 to 1.0; and / or (BaO+SrO+MgO+ZnO+ZrO 2 ) / Na 2 O is less than 1.0, preferably (BaO+SrO+MgO+ZnO+ZrO 2 ) / Na 2 O is 0.8 or less, and more preferably (BaO+SrO+MgO+ZnO+ZrO 2 ) / Na 2 O is 0.05 to 0.6, and more preferably (BaO+SrO+MgO+ZnO+ZrO 2 ) / Na 2 O is 0.1 to 0.5;
[0012] and / or (BaO+WO 3 ) / K 2 O is 1.5 or less, preferably (BaO+WO 3 ) / K 2 O is 1.0 or less, and more preferably (BaO+WO 3 ) / K 2 O is 0.05 to 0.7, and more preferably (BaO+WO 3 ) / K 2 O is 0.1 to 0.5; and / or WO 3 / CaO is less than 0.9, preferably WO 3 / CaO is 0.7 or less, more preferably WO 3 / CaO is 0.5 or less, and WO is more preferably 3 / CaO is less than 0.3; and / or
[0013] (B 2 O 3 +SiO 2 +Al 2 O 3 +WO3 +ZnO+ZrO 2 +Ln 2 O 3 +Bi 2 O 3 ) / (BaO+CaO) is 1.7 or less, preferably (B 2 O 3 +SiO 2 +Al 2 O 3 +WO 3 +ZnO+ZrO 2 +Ln 2 O 3 +Bi 2 O 3 ) / (BaO+CaO) is 1.0 or less, and more preferably (B 2 O 3 +SiO 2 +Al 2 O 3 +WO 3 +ZnO+ZrO 2 +Ln 2 O 3 +Bi 2 O 3 ) / (BaO+CaO) is 0.7 or less, and more preferably (B 2 O 3 +SiO 2 +Al 2 O 3 +WO 3 +ZnO+ZrO 2 +Ln 2 O 3 +Bi 2 O 3 ) / (BaO+CaO) is 0.1 to 0.6, and the Ln 2 O 3 For La 2 O 3 , Gd 2 O 3 , Y 2 O 3 , Yb 2 O 3 One or more of .
[0014] (7) The high-refractive and high-dispersion optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: 2 O 5 : 22-32%, preferably P 2 O 5 :25~29%;and / or Nb2 O 5 : 40-50%, preferably Nb 2 O 5 : 42-47%; and / or TiO 2 : 11-20%, preferably TiO 2 :13~18%;and / or Na 2 O: 2-10%, preferably Na 2 O: 3-8%; and / or K 2 O: 0.5-8%, preferably K 2 O: 1-6%; and / or BaO: greater than 0 but less than or equal to 6%, preferably BaO: 0.1-3.5%; and / or CaO: 0-6%, preferably CaO: 0.1-4%; and / or MgO: 0-3%, preferably MgO: 0-1%, more preferably MgO is not contained; and / or SrO: 0-3%, preferably SrO: 0-1%, more preferably SrO is not contained; and / or Li 2 O: 0-4%, preferably Li 2 O: 0-2%, preferably no Li 2 O; and / or SiO 2 : 0-3%, preferably SiO 2 :0~1%;and / or B 2 O 3 : 0-3%, preferably B 2 O 3 :0~1.5%;and / or ZrO 2 : 0-3%, preferably ZrO 2 : 0 to 1%, preferably no ZrO 2 ; and / or Al 2 O 3 : 0-3%, preferably Al 2 O 3 : 0 to 1%, preferably no Al 2 O 3 ; and / or ZnO: 0-3%, preferably ZnO: 0-1%, more preferably no ZnO; and / or WO 3 : 0-3%, preferably WO 3 : 0 to 1%, preferably no WO 3 ; and / or Ln 2 O 3 : 0-3%, preferably Ln 2 O 3 : 0 to 1%, preferably no Ln 2 O 3 ; and / or Bi 2 O 3 : 0-3%, preferably Bi 2 O3 : 0 to 1%, preferably no Bi 2 O 3 and / or clarifier: 0 to 0.5%, preferably clarifier: 0 to 0.1%, the Ln 2 O 3 For La 2 O 3 , Gd 2 O 3 , Y 2 O 3 , Yb 2 O 3 One or more of the following, the clarifier is Sb 2 O 3 SnO 2 , SnO, CeO 2 One or more of .
[0015] (8) The refractive index n of the high-refractive and high-dispersion optical glass according to any one of (1) to (4) d is 1.895 to 1.95, preferably 1.90 to 1.95, more preferably 1.91 to 1.94, and further preferably 1.915 to 1.93; Abbe number ν d It is 15 to 22, preferably 16 to 21, more preferably 17 to 20, and further preferably 17.5 to 19.5.
[0016] (9) The thermal expansion coefficient α of the high-refractive and high-dispersion optical glass according to any one of (1) to (4) 100 / 300℃ 100×10 -7 / K or less, preferably 90×10 -7 / K or less, more preferably 85×10 -7 / K or less; and / or acid resistance stability D A 2 or more, preferably 1; and / or water resistance stability D W Two or more types, preferably one type; and / or a transition temperature T g 680°C or less, preferably 670°C or less, more preferably 665°C or less, and further preferably 660°C or less; and / or abrasion degree F A is 160 to 220, preferably 170 to 210, more preferably 180 to 200; and / or density ρ is 3.80 g / cm 3 Below, preferably 3.70g / cm 3 Below, more preferably 3.60g / cm 3 Below, more preferably 3.50 g / cm 3 Below; and / or 70 450nm or less, preferably λ 70445nm or less, more preferably λ 70 is 440nm or less; and / or the weather resistance CR is 2 or more, preferably 1; and / or the Young's modulus E is 9000×10 7 Pa or more, preferably 9500×10 7 Pa or more, more preferably 9800×10 7 Pa or more, more preferably 10000×10 7 Pa~11000×10 7 Pa; and / or the bubble degree is above grade A, preferably A 0 Grade A or above, preferably A 00 and / or the stripe degree is C level or above, preferably B level or above; and / or the secondary pressing anti-crystallization performance is C level or above, preferably B level or above, more preferably A level.
[0017] (10) A glass preform is made of the high-refractive and high-dispersion optical glass described in any one of (1) to (9).
[0018] (11) An optical element is made of the high-refractive and high-dispersion optical glass described in any one of (1) to (9), or is made of the glass preform described in (10).
[0019] (12) An optical instrument comprising the high-refractive and high-dispersion optical glass described in any one of (1) to (9), or an optical element described in (11).
[0020] The beneficial effect of the present invention is that, through reasonable component design, the optical glass of the present invention has high refraction and high dispersion as well as low thermal expansion coefficient. DETAILED DESCRIPTION
[0021] The following is a detailed description of the embodiments of the high-refractive and high-dispersion optical glass of the present invention, but the present invention is not limited to the following embodiments, and can be implemented by appropriate changes within the scope of the purpose of the present invention. In addition, although there are cases where the repeated description is appropriately omitted, the main purpose of the invention is not limited thereto. In the following content, the high-refractive and high-dispersion optical glass of the present invention is sometimes referred to as optical glass or glass.
[0022] [High refractive and high dispersion optical glass]
[0023] The following is an explanation of the range of each component (ingredient) of the optical glass of the present invention. In the present invention, unless otherwise specified, the content, total content, and total content of each component are all expressed in weight percentage (wt%), that is, the content, total content, and total content of each component are expressed in weight percentage relative to the total amount of glass material converted into oxide composition. Here, the "composition converted into oxide" means that when the oxides, complex salts, hydroxides, etc. used as raw materials for the optical glass components of the present invention decompose and transform into oxides during melting, the total amount of the oxide material is taken as 100%.
[0024] Unless otherwise specified in specific circumstances, the numerical ranges listed in the present invention include upper and lower limits, "above" and "below" include endpoint values, and all integers and fractions included in the range, without being limited to the specific values listed when the range is defined. "And / or" referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.
[0025] <Essential Components and Optional Components>
[0026] P 2 O 5 It is the network generator of the glass of the present invention. Compared with silicate glass, phosphate glass can be melted at a low temperature, which is beneficial to improve the light transmittance of the glass. 2 O 5 If the content of P is too high, the viscosity-temperature curve of the glass in the molding area will become flatter, which will slow down the cooling and solidification process of the glass during molding. This is very unfavorable for the molding of large-sized glass. 2 O 5 It is easy to volatilize, which is not conducive to obtaining a good stripe degree of the glass. 2 O 5 The content of P is 20 to 34%, preferably 22 to 32%, and more preferably 25 to 29%. 2 O 5 The content may be 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, 25%, 25.5%, 26%, 26.5%, 27%, 27.5%, 28%, 28.5%, 29%, 29.5%, 30%, 30.5%, 31%, 31.5%, 32%, 32.5%, 33%, 33.5%, 34%.
[0027] Nb 2 O 5 It is a high-refractive and high-dispersion component that can improve the refractive index and chemical stability of the glass. In the present invention, by containing more than 38% Nb2 O 5 In order to obtain the above effects, Nb is preferably 2 O 5 The content of Nb is 40% or more, more preferably 42% or more. 2 O 5 If the content of Nb is too high, the anti-crystallization performance of the glass will decrease and the density will increase. 2 O 5 The upper limit of the content of Nb is 53%, preferably 50%, and more preferably 47%. 2 O 5 The content may be 38%, 38.5%, 39%, 39.5%, 40%, 40.5%, 41%, 41.5%, 42%, 42.5%, 43%, 43.5%, 44%, 44.5%, 45%, 45.5%, 46%, 46.5%, 47%, 47.5%, 48%, 48.5%, 49%, 49.5%, 50%, 50.5%, 51%, 51.5%, 52%, 52.5%, 53%.
[0028] In some embodiments, controlling P 2 O 5 The content of Nb 2 O 5 The ratio between the contents of 2 O 5 / Nb 2 O 5 In the range of 0.4 to 0.85, the glass can more easily obtain the desired optical constants, while optimizing the bubble degree of the glass and reducing the thermal expansion coefficient of the glass. 2 O 5 / Nb 2 O 5 0.4 to 0.85, more preferably P 2 O 5 / Nb 2 O 5 is 0.45 to 0.8, and more preferably P 2 O 5 / Nb 2 O 5 is 0.5 to 0.7, and more preferably P 2 O 5 / Nb 2 O 5 In some embodiments, P 2 O 5 / Nb 2 O 5The value of can be 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.5, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.6, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.7, 0.71, 0.72, 0.73, 0.74, 0.75, 0.76, 0.77, 0.78, 0.79, 0.8, 0.81, 0.82, 0.83, 0.84, 0.85.
[0029] TiO 2 It has the effect of increasing the refractive index and dispersion of glass and improving the resistance to devitrification. The present invention contains an appropriate amount of TiO 2 The glass can be made more stable and the high temperature viscosity of the glass can be reduced. 2 To achieve the above effect, it is preferred to contain more than 11% TiO 2 , more preferably containing more than 13% TiO 2 If TiO 2 The content of TiO exceeds 22%, the tendency of glass crystallization and coloring increases, and the transition temperature rises. 2 The content of TiO is 22% or less, preferably 20% or less, and more preferably 18% or less. 2 The content may be 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%, 20.5%, 21%, 21.5%, 22%.
[0030] In some embodiments, TiO 2 The content of Nb 2 O 5 The ratio between the content of TiO 2 / Nb 2 O 5 Controlling it within the range of 0.2 to 0.55 can improve the weather resistance and Young's modulus of the glass while preventing the transmittance of the glass from decreasing. 2 / Nb 2 O 5 0.2 to 0.55, more preferably TiO 2 / Nb 2 O 5is 0.2 to 0.5, and TiO is more preferred 2 / Nb 2 O 5 In some embodiments, TiO 2 / Nb 2 O 5 The value of can be 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.5, 0.51, 0.52, 0.53, 0.54, 0.55.
[0031] Na 2 O has the effect of improving the melting point and light transmittance of glass, and can also reduce the transition temperature of glass. 2 If the content of O is too high, the chemical stability and weather resistance of the glass will decrease. 2 The content of O is 1 to 12%, preferably 2 to 10%, and more preferably 3 to 8%. 2 The O content can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%.
[0032] K 2 O has the effect of improving the devitrification resistance and melting property of glass. If its content is too high, it is difficult for the glass to obtain the desired high refractive index and high dispersion performance. 2 The content of O is 0 to 10%, preferably 0.5 to 8%, and more preferably 1 to 6%. 2 The O content may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%.
[0033] In some embodiments, controlling TiO 2 The content of K 2 The ratio of O content to TiO 2 / K 2O in the range of 1.0 to 18.0 can improve the weather resistance and secondary compression resistance of the glass. 2 / K 2 O is 1.0 to 18.0, and more preferably TiO 2 / K 2 O is 1.0 to 12.0. Further, TiO 2 / K 2 O is within the range of 1.5 to 10.0, the Young's modulus of the glass can be further optimized. Therefore, TiO 2 / K 2 O is 1.5 to 10.0, and more preferably TiO 2 / K 2 O is 2.0 to 8.0. In some embodiments, TiO 2 / K 2 The value of O can be 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0, 10.5, 11.0, 11.5, 12.0, 12.5, 13.0, 13.5, 14.0, 14.5, 15.0, 15.5, 16.0, 16.5, 17.0, 17.5, 18.0.
[0034] Li 2 O can reduce the transition temperature of glass, but its high content is not good for the acid resistance and thermal expansion coefficient of glass, and it can corrode the melting container (such as platinum crucible). 2 The content of O is 6% or less, preferably 4% or less, and more preferably 2% or less. In some embodiments, it is further preferred that Li 2 O. In some embodiments, Li 2 The O content may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, or 6%.
[0035] BaO can improve the devitrification resistance and light transmittance of the glass in the present invention, and improve the secondary compression molding anti-crystallization performance of the glass. If the BaO content is too high, the chemical stability of the glass will deteriorate and the density will increase. Therefore, the BaO content is 0 to 8%, preferably greater than 0 but less than or equal to 6%, and more preferably 0.1 to 3.5%. In some embodiments, the BaO content can be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%.
[0036] In some embodiments, controlling Nb 2 O 5 、Na 2 Total content of O and BaO Nb 2 O 5 +Na 2 O+BaO and TiO 2 The ratio between the contents of 2 O 5 +Na 2 O+BaO) / TiO 2 In the range of 1.8 to 5.5, the bubble and striae of the glass can be improved, and the thermal expansion coefficient can be prevented from increasing. 2 O 5 +Na 2 O+BaO) / TiO 2 is 1.8 to 5.5, more preferably (Nb 2 O 5 +Na 2 O+BaO) / TiO 2 is 2.0 to 5.0, and more preferably (Nb 2 O 5 +Na 2 O+BaO) / TiO 2 In some embodiments, (Nb 2 O 5 +Na 2 O+BaO) / TiO 2 The value of can be 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5.
[0037] In some embodiments, TiO 2 and K 2 Total content of OTiO 2 +K 2 O with BaO and Na 2 Total content of OBaO+Na 2 The ratio of TiO 2 +K 2 O) / (BaO+Na 2 O) is controlled within the range of 1.6 to 12.0, which can reduce the thermal expansion coefficient of the glass and increase the bubble degree of the glass. 2 +K 2 O) / (BaO+Na 2 O) is 1.6 to 12.0, and more preferably (TiO 2 +K 2 O) / (BaO+Na 2 O) is 2.0 to 10.0. Further, control (TiO 2 +K 2 O) / (BaO+Na 2 O) in the range of 2.2 to 7.0 can further optimize the abrasiveness of the glass. 2 +K 2 O) /
[0038] (BaO+Na 2 O) is 2.2 to 7.0, and more preferably (TiO 2 +K 2 O) / (BaO+Na 2 In some embodiments, (TiO 2 +K 2 O) / (BaO+Na 2 O) can have a value of 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0, 10.5, 11.0, 11.5, 12.0.
[0039] SrO can improve the resistance of glass to devitrification and improve the melting performance of glass, but if its content is too high, the refractive index of the glass will be difficult to meet the design requirements, and the cost of the glass will also rise rapidly. Therefore, the content of SrO is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that SrO is not contained. In some embodiments, the content of SrO may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0040] CaO helps to improve the light transmittance and density of the glass, but when the content of CaO is too much, it will make it difficult for the optical constants of the glass to meet the design requirements, and the anti-crystallization performance will deteriorate. Therefore, the content of CaO is 0-8%, preferably 0-6%, and more preferably 0.1-4%. In some embodiments, the content of CaO may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%.
[0041] In some embodiments, the ratio of CaO content to BaO content CaO / BaO is controlled within the range of 0.1 to 10.0, which can reduce the density of the glass while improving the chemical stability and secondary compression molding anti-crystallization performance of the glass. Therefore, preferably CaO / BaO is 0.1 to 10.0, more preferably CaO / BaO is 0.2 to 7.0, further preferably CaO / BaO is 0.3 to 5.0, and further preferably CaO / BaO is 0.5 to 3.0. In some embodiments, the value of CaO / BaO can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0.
[0042] MgO can reduce the relative partial dispersion of glass, but when the MgO content is too high, the refractive index of the glass is difficult to meet the design requirements, and the anti-crystallization performance and stability of the glass are reduced. Therefore, the content of MgO is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that MgO is not contained. In some embodiments, the content of MgO may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0043] SiO2 It is beneficial to improve the molding viscosity of glass, improve the striation degree of glass, and use quartz crucible to prepare clinker to avoid platinum contamination, thereby improving the transmittance of glass. 2 Too high a content of SiO will increase the glass melting temperature and glass transition temperature. 2 The content of SiO is 0-5%, preferably 0-3%, and more preferably 0-1%. 2 The content may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%.
[0044] B 2 O 3 It can improve the stability and melting property of glass. If its content is too high, the refractive index of glass will be reduced and the anti-crystallization performance of secondary pressing will be deteriorated. 2 O 3 The content of B is 5% or less, preferably 3% or less, and more preferably 1.5% or less. 2 O 3 The content may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%.
[0045] In some embodiments, control B 2 O 3 、SiO 2 Total content B 2 O 3 +SiO 2 The ratio of the content of CaO to the content of 2 O 3 +SiO 2 ) / CaO is below 2.8, which can improve the glass's stripe degree and prevent the glass's secondary pressing anti-crystallization performance from decreasing. 2 O 3 +SiO 2 ) / CaO is 2.8 or less, and more preferably (B 2 O 3 +SiO 2 ) / CaO is 0.1 to 2.0. Further, control (B 2 O 3 +SiO 2 ) / CaO is in the range of 0.2 to 1.5, which can further optimize the weather resistance and coloring of the glass. 2 O 3 +SiO2 ) / CaO is 0.2 to 1.5, and more preferably (B 2 O 3 +SiO 2 ) / CaO is 0.4 to 1.0. In some embodiments, (B 2 O 3 +SiO 2 ) / CaO can have a value of 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8.
[0046] ZrO 2 It can increase the refractive index of glass and adjust the dispersion, improve the anti-crystallization performance and strength of glass. 2 If the content of ZrO is too high, the glass will be more difficult to melt, the melting temperature will rise, and even inclusions will appear inside the glass and the transmittance will decrease. 2 The content is 5% or less, preferably 3%, and more preferably 1% or less. In some embodiments, it is further preferred that ZrO is not contained. 2 In some embodiments, ZrO 2 The content may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%.
[0047] Al 2 O 3 It can improve the chemical stability of glass, but when its content exceeds 5%, the melting property and light transmittance of glass deteriorate. 2 O 3 The content of Al is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that Al is not contained. 2 O 3 In some embodiments, Al 2 O 3 The content may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%.
[0048] ZnO can lower the transition temperature of glass, improve the chemical stability of glass, and reduce the high temperature viscosity of glass. If the ZnO content is too high, the anti-crystallization performance of the glass will deteriorate, and devitrification will easily occur due to the low viscosity. Therefore, the content of ZnO in the present invention is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that ZnO is not contained. In some embodiments, the content of ZnO may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0049] In some embodiments, BaO, SrO, MgO, ZnO, ZrO 2 The total content of BaO+SrO+MgO+ZnO+ZrO 2 with Na 2 The ratio of the content of O (BaO+SrO+MgO+ZnO+ZrO 2 ) / Na 2 O is below 1.0, which can increase the glass's striation and improve the glass's abrasiveness. Therefore, (BaO+SrO+MgO+ZnO+ZrO) is preferred. 2 ) / Na 2 O is 1.0 or less, and more preferably
[0050] (BaO+SrO+MgO+ZnO+ZrO 2 ) / Na 2 O is 0.8 or less, and more preferably (BaO+SrO+MgO+ZnO+ZrO 2 ) / Na 2 O is 0.05 to 0.6, and more preferably (BaO+SrO+MgO+ZnO+ZrO 2 ) / Na 2 O is 0.1 to 0.5. In some embodiments,
[0051] (BaO+SrO+MgO+ZnO+ZrO 2 ) / Na 2 The value of O can be 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0.
[0052] WO 3It can improve the refractive index and dispersion of glass. If its content is too high, the light transmittance of the glass will decrease and the anti-crystallization performance of secondary pressing will deteriorate. 3 The content of WO is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that WO 3 In some embodiments, WO 3 The content may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%.
[0053] In some embodiments, BaO, WO 3 Total content of BaO+WO 3 With K 2 The ratio of the content of O (BaO+WO 3 ) / K 2 O is below 1.5, which can reduce the density of glass and prevent the glass transition temperature from rising. Therefore, (BaO+WO 3 ) / K 2 O is 1.5 or less, more preferably (BaO+WO 3 ) / K 2 O is less than 1.0. Further, control (BaO+WO 3 ) / K 2 O is within the range of 0.05 to 0.7, the fringe degree and Young's modulus of the glass can be further optimized. Therefore, (BaO+WO 3 ) / K 2 O is 0.05 to 0.7, and more preferably (BaO+WO 3 ) / K 2 O is 0.1 to 0.5. In some embodiments, (BaO+WO 3 ) / K 2 The value of O can be 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5.
[0054] In some embodiments, WO 3 The ratio of WO to CaO 3 Controlling WO / CaO below 0.9 can improve the anti-devitrification and chemical stability of the glass. 3 / CaO is 0.9 or less, more preferably WO 3 / CaO is 0.7 or less, and WO is more preferably 3 / CaO is less than 0.5, and WO is more preferred 3 / CaO is less than 0.3. In some embodiments, WO 3 The value of / CaO can be 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, and 0.9.
[0055] Ln 2 O 3 (Ln 2 O 3 For La 2 O 3 , Gd 2 O 3 , Y 2 O 3 , Yb 2 O 3 One or more of these) are components that increase the refractive index and chemical stability of the glass. 2 O 3 The content of Ln is controlled to be less than 5%, which can prevent the devitrification resistance of the glass from decreasing. 2 O 3 The upper limit of the content is 3%, and the more preferred upper limit is 1%. In some embodiments, it is further preferred that Ln 2 O 3 In some embodiments, Ln 2 O 3 The content may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%.
[0056] Bi 2 O 3 It can improve the water resistance of glass and reduce the transition temperature, but if its content is too high, the light transmittance of the glass will decrease, the abrasion resistance and chemical stability will deteriorate, and the density will increase significantly. 2 O 3 The content of Bi is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 1%. In some embodiments, it is further preferred that Bi is not contained. 2 O 3 In some embodiments, Bi 2 O 3The content may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%.
[0057] In some embodiments, B 2 O 3 、SiO 2 、Al 2 O 3 , WO 3 、ZnO、ZrO 2 , Ln 2 O 3 、Bi 2 O 3 The ratio of the total content of BaO to the total content of BaO and CaO (BaO + CaO) 2 O 3 +SiO 2 +Al 2 O 3 +WO 3 +ZnO+ZrO 2 +Ln 2 O 3 +Bi 2 O 3 ) / (BaO+CaO) is controlled below 1.7, which can improve the glass's striation and optimize the glass's abrasiveness. 2 O 3 +SiO 2 +Al 2 O 3 +WO 3 +ZnO+ZrO 2 +Ln 2 O 3 +Bi 2 O 3 ) / (BaO+CaO) is 1.7 or less, and more preferably (B 2 O 3 +SiO 2 +Al 2 O 3 +WO 3 +ZnO+ZrO 2 +Ln 2 O 3 +Bi 2 O 3 ) / (BaO+CaO) is 1.0 or less, and more preferably (B 2 O 3 +SiO 2 +Al 2 O 3 +WO3 +ZnO+ZrO 2 +Ln 2 O 3 +Bi 2 O 3 ) / (BaO+CaO) is 0.7 or less, and more preferably (B 2 O 3 +SiO 2 +Al 2 O 3 +WO 3 +ZnO+ZrO 2 +Ln 2 O 3 +Bi 2 O 3 ) / (BaO+CaO) is 0.1 to 0.6. In some embodiments,
[0058] (B 2 O 3 +SiO 2 +Al 2 O 3 +WO 3 +ZnO+ZrO 2 +Ln 2 O 3 +Bi 2 O 3 ) / (BaO+CaO) can have a value of 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7.
[0059] In the present invention, 0 to 1% Sb is contained 2 O 3 SnO 2 , SnO, CeO 2One or more components in the glass can be used as a clarifier to improve the clarification effect of the glass and the bubble degree of the glass. The content of the clarifier is preferably 0-0.5%, and the content of the clarifier is more preferably 0-0.1%. Since the types and contents of the components of the optical glass of the present invention are reasonably designed and the bubble degree is excellent, it is further preferred in some embodiments that no clarifier is contained. In some embodiments, the content of the clarifier can be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%.
[0060] <Components that should not be contained>
[0061] In the glass of the present invention, even if oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo are contained alone or in combination in small amounts, the glass will be colored and absorption will occur at specific wavelengths in the visible light region, thereby weakening the property of the present invention of improving the visible light transmittance. Therefore, it is preferably substantially free of oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo, especially for optical glasses that require transmittance at wavelengths in the visible light region.
[0062] The oxides of Th, Cd, Tl, Os, Be and Se have a tendency to be controlled in recent years as harmful chemical substances, and environmental protection measures are necessary not only in the manufacturing process of glass, but also in the processing process and the disposal after productization. Therefore, in the case of paying attention to the impact on the environment, it is preferred that they are not actually contained except for being inevitably mixed in. Thus, the optical glass does not actually contain substances that pollute the environment. Therefore, even if special environmental countermeasures are not taken, the optical glass of the present invention can be manufactured, processed and discarded.
[0063] In order to achieve environmental friendliness, the optical glass of the present invention preferably does not contain As 2 O 3 and PbO.
[0064] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the optical glass of the present invention; however, as raw materials and / or equipment for producing optical glass, there will be certain impurities or components that are not intentionally added, which will be contained in a small amount or trace amount in the final optical glass, and this situation is also within the scope of protection of the patent of this invention.
[0065] Next, the properties of the high-refractive and high-dispersion optical glass of the present invention will be described.
[0066] <Refractive Index and Abbe Number>
[0067] The refractive index of optical glass (n d ) and the Abbe number (νd ) Tested according to the method specified in GB / T 7962.1-2010.
[0068] In some embodiments, the refractive index (n d ) has a lower limit of 1.895, a preferred lower limit is 1.90, a more preferred lower limit is 1.91, and a further preferred lower limit is 1.915.
[0069] In some embodiments, the refractive index (n d ) is 1.95, preferably 1.94, and more preferably 1.93.
[0070] In some embodiments, the Abbe number (ν d ) has a lower limit of 15, a preferred lower limit of 16, a more preferred lower limit of 17, and a further preferred lower limit of 17.5.
[0071] In some embodiments, the Abbe number (ν d ) has an upper limit of 22, a preferred upper limit of 21, a more preferred upper limit of 20, and a further preferred upper limit of 19.5.
[0072] <Coefficient of Thermal Expansion>
[0073] Thermal expansion coefficient of optical glass (α 100 / 300℃ ) Test data at 100-300℃ according to the method specified in GB / T7962.16-2010.
[0074] In some embodiments, the thermal expansion coefficient (α 100 / 300℃ ) is 100×10 -7 / K or less, preferably 90×10 -7 / K or less, more preferably 85×10 -7 / K or less.
[0075] <Acid resistance stability>
[0076] Acid resistance stability of optical glass (D A ) (Powder method) Tested in accordance with the method specified in GB / T 17129.
[0077] In some embodiments, the acid resistance stability (D A ) is 2 or more types, preferably 1 type.
[0078] <Water resistance stability>
[0079] Water resistance stability of optical glass (D W ) (Powder method) Tested in accordance with the method specified in GB / T 17129.
[0080] In some embodiments, the water resistance stability (D W ) is 2 or more types, preferably 1 type.
[0081] <Transition Temperature>
[0082] Transition temperature of optical glass (T g ) Tested according to the method specified in GB / T7962.16-2010.
[0083] In some embodiments, the transition temperature (T g ) is 680°C or lower, preferably 670°C or lower, more preferably 665°C or lower, and further preferably 660°C or lower.
[0084] <Abrasion>
[0085] Abrasiveness of optical glass (F A ) refers to the value obtained by multiplying the ratio of the wear volume of the sample to the wear volume (volume) of the standard sample (H-K9 glass) under exactly the same conditions by 100, and is expressed by the following formula:
[0086]
[0087] Where: V—volume wear of the sample being tested;
[0088] V 0 —Volume loss of standard sample;
[0089] W—mass wear loss of the sample being tested;
[0090] W 0 —Abrasion loss of standard sample mass;
[0091] ρ—density of the sample being tested;
[0092] ρ 0 —Standard sample density.
[0093] In some embodiments, the abrasion degree (F A ) has a lower limit of 160, a preferred lower limit of 170, and a more preferred lower limit of 180.
[0094] In some embodiments, the abrasion degree (F A ) has an upper limit of 220, a preferred upper limit of 210, and a more preferred upper limit of 200.
[0095] <density>
[0096] The density (ρ) is tested according to the method specified in GB / T7962.20-2010.
[0097] In some embodiments, the density (ρ) of the high refractive and high dispersion optical glass of the present invention is 3.80 g / cm 3 Below, preferably 3.70g / cm 3 Below, more preferably 3.60g / cm 3 Below, more preferably 3.50 g / cm 3 the following.
[0098] <Color>
[0099] The short-wave transmission spectrum characteristics of the glass of the present invention are expressed by the coloration (λ 70 ) indicates. 70 It refers to the wavelength when the glass transmittance reaches 70%. 70 The measurement is to use a glass with a thickness of 10±0.1mm and two opposite planes parallel to each other and optically polished, and measure the spectral transmittance in the wavelength range from 280nm to 700nm and the wavelength at which the transmittance is 70%. The so-called spectral transmittance or transmittance is the wavelength at which the incident intensity I is perpendicular to the above surface of the glass. in Light of intensity I passes through the glass and emerges from a plane out The light of the case through I out / I in The amount expressed by λ also includes the transmittance of the surface reflection loss on the above surface of the glass. The higher the refractive index of the glass, the greater the surface reflection loss. Therefore, in high refractive index glass, λ 70 A small value of means that the glass itself is less colored and has a high light transmittance.
[0100] In some embodiments, the high refractive and high dispersion λ of the optical glass of the present invention is 70 450nm or less, preferably λ 70 445nm or less, more preferably λ 70 Below 440nm.
[0101] <Weather resistance>
[0102] The test method for weather resistance (CR) of optical glass is as follows: place the sample in a test box with a saturated water vapor environment of 90% relative humidity, alternately cycle every 1 hour at 40-50°C, and cycle for 15 cycles. The weather resistance category is divided according to the change in turbidity before and after the sample is placed. The weather resistance classification is shown in Table 1:
[0103] Table 1.
[0104]
[0105] In some embodiments, the weather resistance (CR) of the high-refractive and high-dispersion optical glass of the present invention is Class 2 or higher, preferably Class 1.
[0106] <Young's modulus>
[0107] Young's modulus (E) is calculated using the following formula by ultrasonic testing of its longitudinal wave velocity and transverse wave velocity.
[0108]
[0109] G=V S 2 ρ
[0110] Where: E is Young's modulus, Pa;
[0111] G is the shear modulus, Pa;
[0112] V T is the shear wave velocity, m / s;
[0113] V S is the longitudinal wave velocity, m / s;
[0114] ρ is the glass density, g / cm 3 .
[0115] In some embodiments, the Young's modulus (E) of the high refractive and high dispersion optical glass of the present invention is 9000×10 7 Pa or more, preferably 9500×10 7 Pa or more, more preferably 9800×10 7 Pa or more, more preferably 10000×10 7 Pa~11000×10 7 Pa.
[0116] <Bubble Degree>
[0117] The bubble degree of optical glass is tested according to the method specified in GB / T7962.8-2010.
[0118] In some embodiments, the bubble degree of the high refractive and high dispersion optical glass of the present invention is above grade A, preferably grade A. 0 Grade A or above, preferably A 00 class.
[0119] <Striation Degree>
[0120] The striation degree of the glass of the present invention is tested by the following method: using a striation meter composed of a point light source and a lens, the striation degree is compared with the standard sample from the direction where the striation is most easily visible, and is divided into 4 levels, namely, A, B, C, and D. Level A means no striations visible to the naked eye under the specified test conditions, level B means fine and dispersed striations under the specified test conditions, level C means slight parallel striations under the specified test conditions, and level D means coarse striations under the specified test conditions.
[0121] In some embodiments, the fringe degree of the high-refractive and high-dispersion optical glass of the present invention is C-level or higher, preferably B-level or higher.
[0122] <Secondary Pressing Anti-Crystallization Performance>
[0123] The test method of the secondary pressing anti-crystallization performance is as follows: cut the sample glass into 20×20×10mm specifications and place it in a temperature of T g Keep the glass in a muffle furnace at +(200-250)℃ for 15-30 minutes (the present invention uses 880℃ for 15 minutes), take it out and cool it down, and observe whether there is devitrification or crystal particles on the surface and inside of the glass. If the glass sample has no devitrification and crystal particles, the secondary pressing anti-crystallization performance of the glass is excellent.
[0124] In the secondary pressing anti-crystallization performance test, according to the above-mentioned test method, the glass with no devitrification or crystallization grains on the surface and no crystal particles inside is recorded as "A", the glass with no crystallization grains inside but devitrification or crystallization grains on the surface is recorded as "B" (the devitrification or crystallization grains on the surface of the glass during the secondary pressing can be removed by grinding, but the grinding cost may increase), the glass with 1 to 10 crystal particles inside is recorded as "C", the glass with 10 to 20 crystal particles inside is recorded as "D", and the glass with more than 20 densely packed crystallization particles inside is recorded as "×".
[0125] In some embodiments, the secondary pressing anti-crystallization performance of the high refractive and high dispersion optical glass of the present invention is above Class C, preferably above Class B, and more preferably Class A.
[0126] [Method for producing optical glass]
[0127] The manufacturing method of the high-refractive and high-dispersion optical glass of the present invention is as follows: the glass of the present invention is produced using conventional raw materials and processes, including but not limited to using oxides, hydroxides, complex salts (such as carbonates, nitrates, sulfates, phosphates, metaphosphates, etc.), boric acid, etc. as raw materials, and after mixing according to conventional methods, the prepared furnace materials are put into a melting furnace (such as platinum or platinum alloy crucible) at 1000-1300° C. for melting, and after clarification and homogenization, a homogeneous molten glass without bubbles and undissolved substances is obtained, and the molten glass is cast in a mold and annealed. Those skilled in the art can appropriately select raw materials, process methods and process parameters according to actual needs.
[0128] [Glass preforms and optical components]
[0129] The prepared optical glass can be used to make a glass preform by means of direct drop molding, grinding, or compression molding such as hot press molding. That is, the molten optical glass can be directly precision drop molded into a glass precision preform, or the glass preform can be made by mechanical processing such as grinding and grinding, or the preform for compression molding made of the optical glass can be made by hot press molding and then grinding. It should be noted that the means for preparing the glass preform are not limited to the above means.
[0130] As described above, the optical glass of the present invention is useful for various optical elements and optical designs, and it is particularly preferred to form a preform from the optical glass of the present invention and use the preform to perform re-hot pressing, precision stamping, etc. to produce optical elements such as lenses and prisms.
[0131] The glass preform and optical element of the present invention are both formed of the optical glass of the present invention. The glass preform of the present invention has the excellent properties of optical glass; the optical element of the present invention has the excellent properties of optical glass, and can provide various optical elements such as lenses and prisms with high optical value.
[0132] Examples of the lens include various lenses having spherical or aspherical lens surfaces, such as a concave meniscus lens, a convex meniscus lens, a biconvex lens, a biconcave lens, a plano-convex lens, and a plano-concave lens.
[0133] [Optical instruments]
[0134] The optical element formed by the optical glass of the present invention can be used to manufacture optical instruments such as photographic equipment, video equipment, projection equipment, display equipment, vehicle-mounted equipment and monitoring equipment.
[0135] Example
[0136] <Optical Glass Example>
[0137] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting examples are provided.
[0138] This embodiment adopts the above optical glass manufacturing method to obtain optical glasses having the compositions shown in Tables 2 to 4. In addition, the properties of each glass are measured by the testing method described in the present invention, and the measurement results are shown in Tables 2 to 4.
[0139] Table 2.
[0140]
[0141]
[0142]
[0143] Table 3.
[0144]
[0145]
[0146] Table 4.
[0147]
[0148]
[0149]
[0150] <Glass Preform Example>
[0151] The glass obtained from optical glass examples 1 to 21# is used, for example, by grinding processing, or by molding methods such as hot pressing, precision stamping, etc., to make preforms of various lenses, prisms, etc., such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses.
[0152] <Optical Element Embodiment>
[0153] The preforms obtained in the above-mentioned glass preform embodiments are annealed to reduce the internal stress of the glass and fine-tune the refractive index so that the optical properties such as the refractive index reach the desired values.
[0154] Next, each preform is ground and polished to produce various lenses and prisms such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. The surface of the obtained optical element may be coated with an anti-reflection film.
[0155] <Optical Instrument Embodiment>
[0156] The optical element obtained by the above-mentioned optical element embodiment is optically designed to form an optical component or optical assembly by using one or more optical elements, and can be used in, for example, imaging equipment, sensors, microscopes, medical technology, digital projection, communications, optical communication technology / information transmission, optics / lighting in the automotive field, lithography technology, excimer lasers, wafers, computer chips, and integrated circuits and electronic devices including such circuits and chips.
Claims
1. High refractive and high dispersion optical glass, characterized in that: Its components are expressed in weight percentages and contain: P2O5: 20 - 34%; Nb2O5: 38 - 53%; TiO2: 8 - 22%; Na2O: 1 - 12%, where P2O5 / Nb2O5 is 0.4 - 0.
85.
2. The high-refractive and high-dispersion optical glass according to claim 1, characterized in that: Its components are expressed in weight percentages and also contain: BaO: 0 - 8%; and / or K2O: 0 - 10%; and / or CaO: 0 - 8%; and / or MgO: 0 - 5%; and / or SrO: 0 - 5%; and / or Li2O: 0 - 6%; and / or SiO2: 0 - 5%; and / or B2O3: 0 - 5%; and / or ZrO2: 0 - 5%; and / or Al2O3: 0 - 5%; and / or ZnO: 0 - 5%; and / or WO3: 0 - 5%; and / or Ln2O3: 0 - 5%; and / or Bi2O3: 0 - 5%; and / or clarifying agent: 0 - 1%, where the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and the clarifying agent is one or more of Sb2O3, SnO2, SnO, CeO2.
3. High refractive and high dispersion optical glass, characterized in that: The components include P2O5, Nb2O5, TiO2 and Na2O, and the components are expressed in weight percentage, wherein P2O5 / Nb2O5 is 0.4-0.85, and the refractive index n of the high-refractive and high-dispersion optical glass is d is 1.895~1.95, Abbe number ν d The thermal expansion coefficient is 15 to 22. 100 / 300℃ 100×10 -7 / K or less.
4. The high-refractive and high-dispersion optical glass according to claim 3, characterized in that: Its components are expressed in weight percentages and contain: P2O5: 20 - 34%; and / or Nb2O5: 38 - 53%; and / or TiO2: 8 - 22%; and / or Na2O: 1 - 12%; and / or K2O: 0 - 10%; and / or BaO: 0 - 8%; and / or CaO: 0 - 8%; and / or MgO: 0 - 5%; and / or SrO: 0 - 5%; and / or Li2O: 0 - 6%; and / or SiO2: 0 - 5%; and / or B2O3: 0 - 5%; and / or ZrO2: 0 - 5%; and / or Al2O3: 0 - 5%; and / or ZnO: 0 - 5%; and / or WO3: 0 - 5%; and / or Ln2O3: 0 - 5%; and / or Bi2O3: 0 - 5%; and / or clarifying agent: 0 - 1%, where the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, Yb2O3, and the clarifying agent is one or more of Sb2O3, SnO2, SnO, CeO2.
5. The high-refractive and high-dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: (Nb2O5+Na2O+BaO) / TiO2 is 1.8-5.5, preferably (Nb2O5+Na2O+BaO) / TiO2 is 2.0-5.0, and more preferably (Nb2O5+Na2O+BaO) / TiO2 is 2.5-4.5; and / or P2O5 / Nb2O5 is 0.45-0.8, preferably P2O5 / Nb2O5 is 0.5-0.7, and more preferably P2O5 / Nb2O5 is 0.55-0.65; and / or TiO2 / Nb2O5 is 0.2-0.55, preferably TiO2 / Nb2O5 is 0.2-0.5, and more preferably TiO2 / Nb2O5 is 0.25-0.45; and / or TiO2 / K2O is 1.0-18.0, and preferably Ti O2 / K2O is 1.0-12.0, more preferably TiO2 / K2O is 1.5-10.0, and further preferably TiO2 / K2O is 2.0-8.0; and / or (TiO2+K2O) / (BaO+Na2O) is 1.6-12.0, preferably (TiO2+K2O) / (BaO+Na2O) is 2.0-10.0, more preferably (TiO2+K2O) / (BaO+Na2O) is 2.2-7.0, and further preferably (TiO2+K2O) / (BaO+Na2O) is 2.5-5.5; and / or CaO / BaO is 0.1-10.0, preferably CaO / BaO is 0.2-7.0, more preferably CaO / BaO is 0.3-5.0, and further preferably CaO / BaO is 0.5-3.
0.
6. The high-refractive and high-dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: (B2O3+SiO2) / CaO is less than 2.8, preferably (B2O3+SiO2) / CaO is 0.1-2.0, more preferably (B2O3+SiO2) / CaO is 0.2-1.5, and further preferably (B2O3+SiO2) / CaO is 0.4-1.0; and / or (BaO+SrO+MgO+ZnO+ZrO2) / Na2O is less than 1.0, preferably (BaO+SrO+MgO+ZnO+ZrO2) / Na2O is less than 1.0, a2O is 0.8 or less, more preferably (BaO+SrO+MgO+ZnO+ZrO2) / Na2O is 0.05-0.6, and further preferably (BaO+SrO+MgO+ZnO+ZrO2) / Na2O is 0.1-0.5; and / or (BaO+WO3) / K2O is 1.5 or less, preferably (BaO+WO3) / K2O is 1.0 or less, more preferably (BaO+WO3) / K2O is 0.05-0.7, and further preferably (BaO+WO3) / K2O is 0 .1~0.5; and / or WO3 / CaO is less than 0.9, preferably WO3 / CaO is less than 0.7, more preferably WO3 / CaO is less than 0.5, and further preferably WO3 / CaO is less than 0.3; and / or (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is less than 1.7, preferably (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is less than 1.0, more preferably (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is less than 0.7, further preferably (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is 0.1~0.6, and the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3.
7. The high-refractive and high-dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: P2O5: 22-32%, preferably P2O5: 25-29%; and / or Nb2O5: 40-50%, preferably Nb2O5: 42-47%; and / or TiO2: 11-20%, preferably TiO2: 13-18%; and / or Na2O: 2-10%, preferably Na2O: 3-8%; and / or K2O: 0.5-8%, preferably K2O: 1-6%; and / or BaO: greater than 0 but less than or equal to 6% , preferably BaO: 0.1-3.5%; and / or CaO: 0-6%, preferably CaO: 0.1-4%; and / or MgO: 0-3%, preferably MgO: 0-1%, more preferably MgO is not contained; and / or SrO: 0-3%, preferably SrO: 0-1%, more preferably SrO is not contained; and / or Li2O: 0-4%, preferably Li2O: 0-2%, more preferably Li2O is not contained; and / or SiO2: 0-3%, preferably SiO2: 0-1%; and / or or B2O3: 0-3%, preferably B2O3: 0-1.5%; and / or ZrO2: 0-3%, preferably ZrO2: 0-1%, more preferably no ZrO2; and / or Al2O3: 0-3%, preferably Al2O3: 0-1%, more preferably no Al2O3; and / or ZnO: 0-3%, preferably ZnO: 0-1%, more preferably no ZnO; and / or WO3: 0-3%, preferably WO3: 0-1%, more preferably no WO3; and / or L n2O3: 0-3%, preferably Ln2O3: 0-1%, more preferably no Ln2O3; and / or Bi2O3: 0-3%, preferably Bi2O3: 0-1%, more preferably no Bi2O3; and / or clarifier: 0-0.5%, preferably clarifier: 0-0.1%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
8. The high-refractive and high-dispersion optical glass according to any one of claims 1 to 4, characterized in that: The refractive index n of the high-refractive and high-dispersion optical glass is d is 1.895 to 1.95, preferably 1.90 to 1.95, more preferably 1.91 to 1.94, and further preferably 1.915 to 1.93; Abbe number ν d It is 15 to 22, preferably 16 to 21, more preferably 17 to 20, and further preferably 17.5 to 19.
5.
9. The high-refractive and high-dispersion optical glass according to any one of claims 1 to 4, characterized in that: The thermal expansion coefficient α of the high-refractive and high-dispersion optical glass 100 / 300℃ 100×10 -7 / K or less, preferably 90×10 -7 / K or less, more preferably 85×10 -7 / K or less; and / or acid resistance stability D A 2 or more, preferably 1; and / or water resistance stability D W Two or more types, preferably one type; and / or a transition temperature T g 680°C or less, preferably 670°C or less, more preferably 665°C or less, and further preferably 660°C or less; and / or abrasion degree F A is 160 to 220, preferably 170 to 210, more preferably 180 to 200; and / or density ρ is 3.80 g / cm 3 Below, preferably 3.70g / cm 3 Below, more preferably 3.60g / cm 3 Below, more preferably 3.50 g / cm 3 Below; and / or 70 450nm or less, preferably λ 70 445nm or less, preferably λ 70 is 440nm or less; and / or the weather resistance CR is 2 or more, preferably 1; and / or the Young's modulus E is 9000×10 7 Pa or more, preferably 9500×10 7 Pa or more, more preferably 9800×10 7 Pa or more, more preferably 10000×10 7 Pa~11000×10 7 Pa; and / or the bubble degree is A grade or above, preferably A0 grade or above, more preferably A 00 and / or the stripe degree is C level or above, preferably B level or above; and / or the secondary pressing anti-crystallization performance is C level or above, preferably B level or above, more preferably A level.
10. A glass preform made of the high-refractive and high-dispersion optical glass according to any one of claims 1 to 9.
11. An optical element, made of the high-refractive and high-dispersion optical glass according to any one of claims 1 to 9, or made of the glass preform according to claim 10.
12. An optical instrument comprising the high-refractive and high-dispersion optical glass according to any one of claims 1 to 9, or an optical element according to claim 11.