Preparation method of continuous flow ultraviolet light chemical reaction quartz glass chip

By performing femtosecond laser modification and high-temperature molten salt etching on the surface of quartz glass, combined with pre-pressure bonding and vacuum annealing, the problems of low corrosion efficiency and low bonding yield in the preparation of quartz glass chips in the prior art are solved. , realizes efficient preparation of large-sized chips, and enhances the pressure tolerance and stability of the chips.

CN118908583APending Publication Date: 2024-11-08COSMICRON (SUZHOU) TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410969677.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing preparation methods for quartz glass microfluidic chips have low corrosion efficiency, poor internal pressure tolerance, inability to prepare large-sized chips, and the strong acids and alkalis used during the corrosion process have safety risks and environmental pollution problems, resulting in low bond yield. and runner closure problem.

Method used

Direct modification of femtosecond laser on the surface of quartz glass, using high-temperature mixed molten salt etching to form a microstructure, followed by pre-pressure bonding and vacuum annealing to form a continuous flow ultraviolet photochemical reaction quartz glass chip, improving corrosion efficiency and bonding Yield, avoid surface shape changes and roughness increases.

Benefits of technology

It improves corrosion efficiency and bond yield, enhances the chip's pressure tolerance, realizes the preparation of large-size chips, reduces safety risks and environmental pollution, and ensures the integrity and stability of the runner.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention discloses a continuous flow ultraviolet light chemical reaction quartz glass chip preparation method, which comprises: carrying out direct writing modification on a quartz glass surface through femtosecond laser, and processing a micro-channel modification region on the quartz glass surface; putting the quartz glass subjected to surface modification into high-temperature mixed fused salt for etching treatment, and then putting the quartz glass into water for boiling until a microstructure appears on the surface of the quartz glass; the microstructures of the two pieces of quartz glass are aligned and attached, and then pre-pressing bonding is carried out; and carrying out annealing treatment on the bonded quartz glass under a vacuum condition to obtain the continuous flow ultraviolet light chemical reaction quartz glass chip. Femtosecond laser direct modification is carried out on the surface of the quartz glass, a modified area is etched through high-temperature fused salt to form a flow channel microstructure, the etching selection ratio reaches up to 1: 500 or above, increase of the surface roughness of the unmodified quartz glass and change of the overall surface type are avoided, and finally the micro-flow-channel quartz glass chip is formed through prepressing bonding. The corrosion efficiency is high, and the bonding yield is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of continuous flow photochemical reaction chips, and in particular to a preparation method of a continuous flow ultraviolet light chemical reaction quartz glass chip. Background Art

[0002] In the prior art, the preparation method of the microfluidic chip used for continuous flow photochemical microreaction synthesis is generally as follows: the inside of the quartz glass is modified by femtosecond laser direct writing, a hole is opened above the modified area, and the corrosive liquid enters the modified area inside the quartz through the opening to corrode the modified area, and the microchannel structure is formed inside the quartz glass. Finally, the opening is sintered and sealed with a carbon dioxide laser to prepare a quartz glass microfluidic chip.

[0003] The quartz glass chip prepared by the above method can be applied to continuous flow photochemical microreactions, but it is only a laboratory product and cannot be mass-produced. At the same time, there are the following problems: 1. The corrosion efficiency of the femtosecond direct writing inside the quartz glass combined with the opening-assisted corrosion is low; 2. The stress of carbon dioxide laser ablation sealing is large, which makes the chip's ability to withstand internal reaction pressure not high, and its application is limited; 3. It is impossible to prepare large-size (such as 4 inches and above) chips, and its application is limited; 4. The corrosion method used for femtosecond direct writing modification of quartz glass generally uses high-concentration hydrofluoric acid and strong potassium oxide aqueous solution, which are strong acids and strong bases, respectively, which have safety risks and are not environmentally friendly. The roughness of the quartz glass after corrosion will increase significantly and the surface shape will change significantly.

[0004] In addition, for quartz glass corroded by strong acid and strong alkali, due to the large changes in roughness and surface shape, if the internal modification by femtosecond direct writing is not adopted, but the surface modification and bonding method is adopted, precision polishing is still required after corrosion. And because of the microstructure on the surface, the surface shape cannot be strictly tested during the precision polishing process, and the surface shape cannot be controlled, so the yield of subsequent bonding is relatively very low, and there is a problem of flow channel closure, and even bonding is impossible. Therefore, there are currently no quartz glass bonding chips on the market. Therefore, it is of great significance to research and develop a preparation method for quartz glass chips with high corrosion efficiency and high bonding yield. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a continuous flow ultraviolet light chemical reaction quartz glass chip, wherein a femtosecond laser is directly modified on the surface of the quartz glass, and a flow channel microstructure is formed by etching the modified area with a molten salt, and the etching selectivity is as high as 1:500 or more, thereby avoiding an increase in the surface roughness of the quartz glass and a change in the surface shape, and finally a microchannel quartz glass chip is formed by pre-pressing and bonding, with high etching efficiency and high bonding yield.

[0006] In order to solve the above technical problems, the present invention provides a method for preparing a continuous flow ultraviolet light chemical reaction quartz glass chip, comprising the following steps:

[0007] S1, performing direct writing modification on the quartz glass surface by femtosecond laser, and processing a microchannel modified area on the quartz glass surface;

[0008] S2, placing the surface-modified quartz glass in a high-temperature mixed molten salt for etching, and then boiling it in water until a microstructure appears on the surface of the quartz glass;

[0009] The mixed molten salt comprises the following components by mass percentage:

[0010] Potassium nitrate 40-50wt%,

[0011] Sodium nitrate 40-50wt%,

[0012] Sodium fluoride 0-10wt%,

[0013] Potassium hydroxide 0-5wt%,

[0014] Sodium hydroxide 0-5wt%;

[0015] S3, aligning and laminating the two quartz glass microstructures, and then performing pre-pressing bonding;

[0016] S4, annealing the bonded quartz glass under vacuum conditions to obtain the continuous flow ultraviolet light chemical reaction quartz glass chip.

[0017] The present invention directly modifies the surface of quartz glass by femtosecond laser, and then etches the modified area of ​​the quartz glass surface by molten salt to form a flow channel microstructure. The reaction area is large, the corrosion efficiency is improved, and more complex microstructures can be made at the same time. The surface etching selectivity is as high as 1:500 or more, which improves the fidelity of the surface shape of the non-direct-written modified part of the quartz glass surface, avoids the increase of the surface roughness of the quartz glass and the change of the surface shape, provides good prerequisites for subsequent bonding, avoids the problem of flow channel closure caused by bonding, and has a high bonding yield. Finally, a microchannel quartz glass chip is formed by pre-pressing bonding, the quartz glass is bonded and fused into one, and the internal microstructure withstands higher pressure.

[0018] Furthermore, in S1, the parameters of the femtosecond laser direct writing modification are: pulse width 50-500fs, frequency 100-500KHz, power 1-10W.

[0019] Furthermore, in S2, the temperature of the mixed molten salt is 350-500° C., and the etching time is 60-240 min.

[0020] Furthermore, in S2, the boiling time is 60-240 min.

[0021] Furthermore, in S2, the quartz glass is cooled to room temperature after etching and then boiled in water.

[0022] Furthermore, in S2, the quartz glass further includes a cleaning step after the microstructure is revealed.

[0023] Furthermore, in S3, the pre-pressure during the pre-pressing and bonding process is 0.1-1 MPa, and the bonding time is 60-300 min.

[0024] Furthermore, in S4, the vacuum degree of the vacuum condition is 1×10 -4 Pa-1×10 -1 Pa.

[0025] Furthermore, in S4, the annealing treatment is specifically: heating to 1050-1150° C. at a heating rate of 5-10° C. / min, and keeping the temperature for 20-40 minutes.

[0026] The second aspect of the present invention provides a continuous flow ultraviolet light chemical reaction quartz glass chip prepared by the preparation method described in the first aspect.

[0027] Beneficial effects of the present invention:

[0028] The present invention directly modifies the surface of quartz glass by femtosecond laser, and then etches the modified area on the surface of quartz glass by molten salt to form a flow channel microstructure, which has a large reaction area, improves the corrosion efficiency, and can make more complex microstructures.

[0029] The surface etching selectivity of the present invention is as high as 1:500 or more, which improves the fidelity of the surface shape of the non-direct writing modified part of the quartz glass surface, avoids the increase of the surface roughness of the quartz glass and the change of the surface shape, provides good prerequisites for subsequent bonding, avoids the problem of flow channel closure caused by bonding, and has a high bonding yield.

[0030] The quartz glass of the present invention is bonded and fused into one body, and the internal microstructure can withstand higher pressure. DETAILED DESCRIPTION

[0031] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0032] Example 1

[0033] S1, using the parameters: pulse width 50fs, frequency 100KHz, power 1W femtosecond laser to directly write channel-type microstructures on the surface of quartz glass;

[0034] S2. Prepare a mixed molten salt, wherein the mixed molten salt comprises the following components by mass percentage:

[0035]

[0036] The molten salt mixed in the above proportion is placed in a corundum crucible, the temperature is raised to 350°C and kept warm, and the quartz glass modified by femtosecond laser direct writing is placed in it for selective etching for 240 minutes, and then taken out and cooled to room temperature;

[0037] S3, putting the quartz glass etched by the mixed molten salt into a beaker filled with tap water, heating the beaker to boil for 240 minutes to reveal the microstructure, and then taking it out and cleaning it;

[0038] S4. In an ultra-clean environment, align the surface microstructure of a piece of quartz glass with the microstructure of another piece of quartz glass and bond them together, then pre-apply a pressure of 0.1 MPa for pre-bonding for 300 minutes.

[0039] S5. Place the pre-bonded quartz glass into a high-temperature annealing furnace and evacuate to 1×10 -1 Pa, and heated to 1100°C at 10°C / min, kept warm for 30min, and then turned off the power and cooled to room temperature with the furnace to obtain a continuous flow ultraviolet light chemical reaction quartz glass chip. The parameters for preparing the quartz glass chip in this embodiment are as follows:

[0040] Category parameter Quartz glass surface etching selectivity 1:500 Liquid holding capacity ≥10 mL Withstand temperature range -70℃-300℃ Withstanding pressure 2MPa Working wavelength 170-350nm light transmittance ≥90%

[0041] Example 2

[0042] S1, using the parameters: pulse width 100fs, frequency 400KHz, power 5W femtosecond laser to directly write channel-type microstructures on the surface of quartz glass;

[0043] S2. Prepare a mixed molten salt, wherein the mixed molten salt comprises the following components by mass percentage:

[0044]

[0045]

[0046] The molten salt mixed in the above proportion is placed in a corundum crucible, the temperature is raised to 400°C and kept warm, and the quartz glass modified by femtosecond laser direct writing is placed in it for selective etching for 180 minutes, and then taken out and cooled to room temperature;

[0047] S3, putting the quartz glass etched by the mixed molten salt into a beaker filled with tap water, heating the beaker to boil for 160 minutes to reveal the microstructure, and then taking it out and cleaning it;

[0048] S4. In an ultra-clean environment, align the surface microstructure of a piece of quartz glass with the microstructure of another piece of quartz glass and bond them together, then pre-apply a pressure of 0.5 MPa for pre-bonding for 200 minutes.

[0049] S5. Place the pre-bonded quartz glass into a high-temperature annealing furnace and evacuate to 1×10 -1 Pa, and heated to 1100°C at 10°C / min, kept warm for 30min, and then turned off the power and cooled to room temperature with the furnace to obtain a continuous flow ultraviolet light chemical reaction quartz glass chip. The parameters for preparing the quartz glass chip in this embodiment are as follows:

[0050] Category parameter Quartz glass surface etching selectivity 1:530 Liquid holding capacity ≥10 mL Withstand temperature range -70℃-300℃ Withstanding pressure 4MPa Working wavelength 170-350nm light transmittance ≥90%

[0051] Example 3

[0052] S1, using the parameters: pulse width 250fs, frequency 300KHz, power 8W femtosecond laser to directly write channel-type microstructures on the surface of quartz glass;

[0053] S2. Prepare a mixed molten salt, wherein the mixed molten salt comprises the following components by mass percentage:

[0054]

[0055]

[0056] The molten salt mixed in the above proportion is placed in a corundum crucible, the temperature is raised to 450°C and kept warm, and the quartz glass modified by femtosecond laser direct writing is placed in it for selective etching for 120 minutes, and then taken out and cooled to room temperature;

[0057] S3, putting the quartz glass etched by the mixed molten salt into a beaker filled with tap water, heating the beaker to boil for 120 minutes to reveal the microstructure, and then taking it out and cleaning it;

[0058] S4. In an ultra-clean environment, align the surface microstructure of a piece of quartz glass with the microstructure of another piece of quartz glass and bond them together, then pre-apply a pressure of 0.8 MPa for pre-bonding for 100 minutes.

[0059] S5. Place the pre-bonded quartz glass into a high-temperature annealing furnace and evacuate to 1×10 -1 Pa, and heated to 1100°C at 10°C / min, kept warm for 30min, and then turned off the power and cooled to room temperature with the furnace to obtain a continuous flow ultraviolet light chemical reaction quartz glass chip. The parameters for preparing the quartz glass chip in this embodiment are as follows:

[0060] Category parameter Quartz glass surface etching selectivity 1:550 Liquid holding capacity ≥10 mL Withstand temperature range -70℃-300℃ Withstanding pressure 5MPa Working wavelength 170-350nm light transmittance ≥90%

[0061] Example 4

[0062] S1, using the femtosecond laser with the parameters of pulse width 500fs, frequency 500KHz, and power 10W to directly write the channel microstructure on the surface of quartz glass;

[0063] S2. Prepare a mixed molten salt, wherein the mixed molten salt comprises the following components by mass percentage:

[0064] Potassium nitrate 50wt%,

[0065] Sodium nitrate 50wt%;

[0066] The molten salt mixed in the above proportion is placed in a corundum crucible, the temperature is raised to 500°C and kept warm, and the quartz glass modified by femtosecond laser direct writing is placed in it for selective etching for 60 minutes, and then taken out and cooled to room temperature;

[0067] S3, putting the quartz glass etched by the mixed molten salt into a beaker filled with tap water, heating the beaker to boil for 60 minutes to reveal the microstructure, and then taking it out and cleaning it;

[0068] S4. In an ultra-clean environment, align the surface microstructure of a piece of quartz glass with the microstructure of another piece of quartz glass and bond them together, then pre-apply a pressure of 1 MPa for pre-bonding for 60 minutes.

[0069] S5. Place the pre-bonded quartz glass into a high-temperature annealing furnace and evacuate to 1×10 -1 Pa, and heated to 1100°C at 10°C / min, kept warm for 30min, and then turned off the power and cooled to room temperature with the furnace to obtain a continuous flow ultraviolet light chemical reaction quartz glass chip. The parameters for preparing the quartz glass chip in this embodiment are as follows:

[0070] Category parameter Quartz glass surface etching selectivity 1:580 Liquid holding capacity ≥10 mL Withstand temperature range -70℃-300℃ Withstanding pressure 6MPa Working wavelength 170-350nm light transmittance ≥90%

[0071] In summary, the present invention directly modifies the surface of quartz glass by femtosecond laser, and then etches the modified area of ​​the surface of quartz glass by molten salt to form a flow channel microstructure. The reaction area is large, the corrosion efficiency is improved, and more complex microstructures can be made at the same time. The surface etching selectivity of the present invention is as high as 1:500 or more, among which Example 4 reaches 1:580, which greatly improves the fidelity of the surface shape of the non-direct-written modified part of the quartz glass surface, avoids the increase of the surface roughness of the quartz glass and the change of the surface shape, provides good prerequisites for subsequent bonding, avoids the problem of flow channel closure caused by bonding, has a high bonding yield, and has a liquid holding capacity of ≥10ml. The quartz glass of the present invention is bonded and fused as one, the structure is stable, and the internal microstructure can withstand higher pressure. The quartz glass chip of Example 4 can withstand a pressure of up to 6MPa.

[0072] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A method for preparing a continuous flow ultraviolet light chemical reaction quartz glass chip, characterized in that: The steps include: S1, performing direct writing modification on the quartz glass surface by femtosecond laser, and processing a microchannel modified area on the quartz glass surface; S2, placing the surface-modified quartz glass in a high-temperature mixed molten salt for etching, and then boiling it in water until a microstructure appears on the surface of the quartz glass; The mixed molten salt comprises the following components by mass percentage: Potassium nitrate 40-50wt%, Sodium nitrate 40-50wt%, Sodium fluoride 0-10wt%, Potassium hydroxide 0-5wt%, Sodium hydroxide 0-5wt%; S3, aligning and laminating the two quartz glass microstructures, and then performing pre-pressing bonding; S4, annealing the bonded quartz glass under vacuum conditions to obtain the continuous flow ultraviolet light chemical reaction quartz glass chip.

2. The method for preparing a continuous flow ultraviolet chemical reaction quartz glass chip according to claim 1, characterized in that: In S1, the parameters of the femtosecond laser direct writing modification are: pulse width 50-500fs, frequency 100-500KHz, power 1-10W.

3. The method for preparing a continuous flow ultraviolet chemical reaction quartz glass chip according to claim 1, characterized in that: In S2, the temperature of the mixed molten salt is 350-500° C., and the etching time is 60-240 min.

4. The method for preparing a continuous flow ultraviolet light chemical reaction quartz glass chip according to claim 1, characterized in that: In S2, the boiling time is 60-240 min.

5. The method for preparing a continuous flow ultraviolet light chemical reaction quartz glass chip according to claim 1, characterized in that: In S2, the quartz glass is cooled to room temperature after etching and then boiled in water.

6. The method for preparing a continuous flow ultraviolet chemical reaction quartz glass chip according to claim 1, characterized in that: In S2, after the quartz glass shows the microstructure, a cleaning step is also included.

7. The method for preparing a continuous flow ultraviolet chemical reaction quartz glass chip according to claim 1, characterized in that: In S3, the pre-pressure during the pre-pressing and bonding process is 0.1-1 MPa, and the bonding time is 60-300 min.

8. The method for preparing a continuous flow ultraviolet chemical reaction quartz glass chip according to claim 1, characterized in that: In S4, the vacuum degree of the vacuum condition is 1×10 -4 Pa-1×10 -1 Pa.

9. The method for preparing a continuous flow ultraviolet chemical reaction quartz glass chip according to claim 1, characterized in that: In S4, the annealing treatment is specifically: heating to 1050-1150°C at a heating rate of 5-10°C / min, and keeping the temperature for 20-40 minutes.

10. A continuous flow ultraviolet light chemical reaction quartz glass chip prepared by the preparation method according to any one of claims 1 to 9.