Preparation and adding method and preparation equipment of roof-contact agent for filling coal mine cemented gangue

By using composite top joint agent in cemented gangue filling materials, combined with the flow-promoting and expansion components, the problem of poor fluidity of cemented gangue filling materials in transportation and underground working surfaces is solved, and low-voltage and safe jointing is achieved Top effect, suitable for complex tunnel conditions.

CN118908621AInactive Publication Date: 2024-11-08SHANXI SHUOTU FILLING MINING TECHNOLOGY CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410949431.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During transportation, the aggregate and cemented gangue filling material are isolated from the cementitious material, resulting in poor fluidity and cannot be leveled. It also produces water secretion and shrinkage when the underground working surface is left to stand, resulting in poor pinching. The existing expansion agent is high. And it is unsafe and cannot effectively solve the problems of long-distance transportation and underground mobility.

Method used

A composite top conjugate is adopted, which contains a flow-promoting component and an expansion component. The flow-promoting component is composed of powder polycarboxylic acid water reducing agent, composite cellulose and sodium thiosulfate, and the expansion component is passed through a coating agent. Delaying expansion time and combining the sustained release function, it is suitable for long-distance conveying and low-level inclination tunnels, with low dosage and safe.

Benefits of technology

The self-leveling and filling volume expansion of cemented gangue filling materials in the underground hole is achieved, which solves the problem of poor top joints and reduces the risk of pipe blocking. It is suitable for complex tunnel conditions, has low dosage and is safe, and has an adjustable expansion rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908621A_ABST
    Figure CN118908621A_ABST
Patent Text Reader

Abstract

The invention discloses a composite roof-contacted agent with expansion and flow promotion functions for filling coal mine cemented gangue and an adding method. According to the top-contacting agent, the problem of poor top-contacting of various filling bodies caused by poor slurry fluidity, high bleeding and large shrinkage in a coal mine filling project is comprehensively solved through the expanding agent, the expanding agent coating agent, the flow promoting agent and the flow promoting agent slow-release agent. Moreover, after being coated, the expanding agent can delay the time of expansion and prevent the problems of pipe blockage and invalid expansion caused by expansion in a pipeline, and the flow promoting agent slow-release agent can continuously release the flow promoting effect and improve the flowability, so that various roof contact problems of coal mine cemented gangue filling projects are comprehensively solved, the mixing amount is low, the use is convenient, and the application prospect is wide. The invention further discloses an adding device of the composite roof-contacted agent with the expansion and flow promotion functions for a cemented gangue filling material preparation system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coal mine filling mining, and in particular to a preparation and adding method of a top-connecting agent for coal mine cemented gangue filling and a preparation device. Background Art

[0002] In order to release the coal pressure from "three below" (under buildings, under water bodies, and under railways), control the post-mining surface subsidence, and at the same time dispose of coal mine solid waste - coal gangue, the filling mining technology using cemented coal gangue as filling material has rapidly become popular in my country's coal mining field. Cemented coal gangue filling materials are generally made of cement, fly ash and other cementing materials as cementing materials, with coal gangue as aggregate. After adding water and stirring, they are transported to the underground working face tunnels over a long distance (up to 6km). After that, the filling material hardens to form a filling body to support the roof, thereby achieving the purpose of no coal pillar residue and no surface subsidence after mining.

[0003] At present, cemented gangue filling materials generally have the problem of poor top connection after hardening, which seriously affects the filling quality and mining safety. This situation is mainly caused by two reasons. First, after the filling materials are prepared on the well, the gangue aggregate and the cementing material slurry are separated during the long-distance transportation process, which leads to poor fluidity of the filling materials after they reach the underground working face, and the unfilled areas are formed in the tunnels with low horizontal inclination angles that cannot self-level. On the other hand, the unfilled areas are formed by the seepage layer generated when the filling materials are stationary on the underground working face and the shrinkage of the filling materials during the hardening process. It can be seen that the reasons for poor top connection are complex. If you want to achieve top connection, you need to solve the fluidity problem of cemented gangue filling materials, as well as the seepage and shrinkage problems at the same time.

[0004] At present, there are related technologies to solve the problem of filling material connection. One type is to prepare a filling material with expansion properties. Invention patents CN109020371B, CN103570316A, and CN101792291B use fly ash, slag and other substances with potential gelling activity as the main materials, add aluminum powder or hydrogen peroxide as an expansion agent, and expand through foaming to achieve the purpose of active connection. However, aluminum powder will react quickly and violently when it encounters water or static electricity, and hydrogen peroxide is a strong oxidant, which is not safe to use in coal mines. Moreover, this expansion filling material is an independent and dedicated filling material, and cannot be mixed to solve the problem of cementing coal gangue filling materials. There are also related invention patents involving expansive admixtures for filling. CN117886564A, CN111978063A, and CN103979815B all use lime, cement clinker, and aluminum paste (or aluminum powder) to prepare expansive agents, which can consolidate coal gangue and expand, thereby achieving top connection. However, the dosage of the above expansive agents is relatively high, generally 10% of the mass of the filling material, and the lowest is 1%-4%. Moreover, none of them considers that the expansive agent will begin to expand in the pipeline during long-distance transportation, resulting in the risk of pipe blockage, and it is also unable to solve the top connection problem caused by the segregation of filling materials and the inability to self-level the underground working surface, resulting in the unfilled area. Summary of the invention

[0005] In view of the above-mentioned technical deficiencies, the first purpose of the present invention is to provide a composite top-jointing agent with low dosage and safe use. The core components of the top-jointing agent are a flow-promoting component and an expansion component. The flow-promoting component mainly enables the filling material to self-level on the underground working surface, solving the problem of top-jointing caused by poor fluidity. The expansion component begins to expand in large quantities after leveling to make up for the surface underfilling area caused by seepage and settlement. The combination of the two can enable the cemented coal gangue filling materials under various conditions to achieve complete top-jointing on the underground working surface. Moreover, the expansion component of the top-jointing agent has a slow-release function, and it will expand rapidly after reaching the underground working surface, and will not expand in large quantities in the transportation pipeline to cause pipe blockage. The flow-promoting component also has a slow-release function, part of which is released during the mixing process to improve pumpability, and part of which is released after reaching the underground working surface to achieve underground self-leveling. It is suitable for cemented coal gangue filling projects in long-distance transportation and low-level inclination tunnels.

[0006] In order to achieve the above technical objectives, the present invention adopts a composite capping agent with both expansion and flow-promoting functions, which is composed of the following components in weight ratio: 10-25% of expansion agent, expansion agent coating agent, 40-60% of flow-promoting agent, and 20-40% of flow-promoting sustained-release agent, wherein the expansion agent coating agent accounts for 5% of the expansion agent.

[0007] Preferably, the flow promoter is composed of 25-35% of powdered polycarboxylate water-reducing agent, 0.5-2% of composite cellulose, and 55-75% of sodium thiosulfate.

[0008] Further preferably, the composite cellulose is prepared by mixing cellulose powders with a viscosity of 20000-50000 and 150000-200000 in a ratio of 7:3. Cellulose with a viscosity of 20000-50000 can play a role in suspending, slurry extraction and water retention, and cellulose with a viscosity of 150000-200000 can play a role in thickening. The slurry prepared by using the two together has a low viscosity and good workability.

[0009] More preferably, the expander and the expander coating agent are first mixed and ground at 70°C to form a modified expander. The expander coating agent will melt at 70°C. Through mixing and grinding, the coating agent forms an isolation film on the surface of the expander to delay the expansion time of the expander.

[0010] More preferably, the expansion component composed of the expansion agent and the expansion agent coating agent can be released after the concentrated expansion time is delayed by 1.0 hour.

[0011] More preferably, the flow promoter sustained-release agent can gradually release the water-reducing effect and extend the working time of the filling material by more than 1 hour.

[0012] More preferably, the top bonding agent is used to cement the coal gangue filling material, and the dosage is 2.0-6.0 kg / m 3 , accounting for 0.1-0.3% of the total mass of the filling material, and the expansion rate can be adjusted within the range of 5%-15%.

[0013] The second object of the present invention is to provide a composite top-jointing agent with both expansion and flow-promoting functions for use in a cemented gangue filling material preparation system, comprising a frame, the frame consisting of an upper frame and a lower frame, wherein the upper frame is provided with a combination of a motor and a reducer, the lower part of the reducer is provided with a storage tank, and the two are connected by a first connecting pipe;

[0014] A metering tank is provided in the lower frame, and the storage tank and the metering tank are connected via a second connecting pipe; a stirring tank is provided at the lower part of the metering tank, and the metering tank and the stirring tank are connected via a third connecting pipe; and a water inlet valve is provided on the outer side of the stirring tank.

[0015] Beneficial effects of the present invention:

[0016] 1. The flow-promoting component of the top-jointing agent of the present invention enables the cemented coal gangue filling material to self-level underground, solving the problem of poor top-joining due to insufficient expansion. The expansion component expands in volume after leveling to actively join the top, solving the problem of poor top-joining due to water seepage and shrinkage. The combined use can solve different types of poor top-joining problems under complex tunnel conditions;

[0017] 2. Under the action of the coating agent, the expansion component in the top joint agent of the present invention expands only after the filling material is transported to the underground working surface for 1 hour, and does not expand in the transportation pipeline. Under the action of the slow-release agent, the flow-promoting component can be continuously released within 1 hour, thereby improving the fluidity of the filling material underground, and is suitable for long-distance pumping and lanes with small horizontal inclination angles;

[0018] 3. The dosage of the top joint agent of the present invention is small, only 0.1% to 0.3%, and the expansion rate can be 5% to 15%;

[0019] 4. Through the adding device provided by the present invention, the adding device of the top bonding agent can be connected to the integrated control and preparation system of the general cemented coal gangue filling material on the well, which is convenient to use. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The figure shows the expansion rate of filling materials at different dosages of top joint agent (%);

[0021] Figure 2 The figure shows the effect of mixing and grinding the expander with or without a coating agent on the expansion rate;

[0022] Figure 3 Shown is the change in flowability of the sustained-release formulation with or without a flow enhancer

[0023] Figure 4 Shown is a schematic diagram of the structural device of the device of the present invention;

[0024] Among them, 1. upper frame; 2. lower frame; 3. motor; 4. reducer; 5. storage tank; 6. first connecting pipe; 7. metering tank; 8. second connecting pipe; 9. mixing tank; 10. third connecting pipe; 11. water inlet valve. DETAILED DESCRIPTION

[0025] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0026] Embodiment 1:

[0027] The capping agent was prepared according to the ratio of 15% expansion component (the expansion agent and the expansion agent coating agent were mixed and ground at 70°C in a ratio of 95:5), 85% flow-promoting component, including 50% flow-promoting agent (50% powdered polycarboxylic acid water-reducing agent, 1.5% composite cellulose, 48.5% sodium thiosulfate), and 35% flow-promoting sustained-release agent. The filling material was prepared using different dosages (2.0kg, 3.0kg, 4.0kg) of the capping agent, and the working performance, expansion performance, and strength performance were tested. It can be seen that the addition of the capping agent greatly increased the initial fluidity of the filling material by 1 / 3, and the fluidity loss after 1 hour (simulating the long-distance pumping process) was only 9%. This is because the flow-promoting sustained-release agent has the effect of continuously and slowly releasing the flow-promoting substance to improve the fluidity, and the expansion component is slowly released after 1 hour. The dosage is 3kg / m 3 The expansion rate of the filling body reaches 7% within 3 hours, and the top joint agent has no adverse effect on the water seepage rate and strength of the filling material.

[0028] Table 1 Filling material mix ratio and performance

[0029]

[0030] refer to Figure 1 It is the expansion rate of filling material under different dosage of top joint agent (%).

[0031] Comparative Example 1

[0032] In order to compare the difference between the expansion agent with the coating agent and without the coating agent, the expansion agent with the coating agent and without the coating agent were used to prepare the top connection agent according to the proportion of Example 1, and the filling material was prepared. The filling material formula was the mix ratio 2 in Example 1, and the performance comparison was as follows. The results showed that the expansion agent without the coating agent reacted too quickly and had a large expansion within 30 minutes. If the pumping time was 30 minutes, the effective expansion after reaching the working surface was reduced, the top connection rate was reduced, and a large number of bubbles were generated in the pipeline. The water in the bubbles caused the slurry to have a 1-hour fluidity reduction, which increased the risk of pipe blockage.

[0033] Table 2 Filling material mix ratio and performance

[0034]

[0035] refer to Figure 2 The effect of mixing and grinding the expander with or without a coating agent on the expansion rate.

[0036] Comparative Example 2

[0037] Based on the top connection agent formula of Example 1, the effects of adding a flow promoter and a slow-release agent to the top connection agent on the filling material are compared. The filling material formula is the ratio 2 in Example 1, and the fluidity changes of the two are compared. The change curve is shown in the figure below. The missing components in the top connection agent without a flow promoter and a slow-release agent are replaced with water. The results show that the filling material prepared by the top connection agent without a flow promoter and a slow-release agent loses its workability quickly, and cannot self-level after reaching the underground working surface, which can easily lead to underfilled areas and affect the top connection. After adding the slow-release agent, the workability of the filling material decreases very little within 1 hour.

[0038] Depend on Figure 4 It can be seen that the present invention also discloses a composite capping agent with both expansion and flow promotion functions, which is used in an adding device of a cemented gangue filling material preparation system, including a frame, which is composed of an upper frame 1 and a lower frame 2, wherein the upper frame 1 is provided with a combination of a motor 3 and a reducer 4, and a storage tank 5 is provided at the lower part of the reducer 4, and the reducer 4 and the storage tank 5 are connected by a first connecting pipe 6.

[0039] A metering tank 7 is provided in the lower frame 2, and the storage tank 5 and the metering tank 7 are connected by a second connecting pipe 8; a stirring tank 9 is provided at the lower part of the metering tank 7, and the metering tank 7 and the stirring tank 9 are connected by a third connecting pipe 10; and a water inlet valve 11 is provided on the outside of the stirring tank 9 to pass into the stirring tank 9.

[0040] When the above device is used, the capping agent is added to the storage tank 5, and the motor 3 and the reducer 4 push the material into the metering tank 7 for metering. The material in the metering tank 7 further enters the mixing tank 9 and is mixed with water to form a slurry, and finally added to the filling material mixing equipment.

[0041] In actual applications, the device can be intelligently connected to the centralized control center of the coal mine filling station to realize computer-controlled addition.

[0042] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A composite capping agent with both expansion and flow-promoting functions. It is characterized in that The invention is composed of the following components in weight ratio: 10-25% of a swelling agent, a swelling agent coating agent, 40-60% of a flow promoter, and 20-40% of a flow promoter sustained-release agent, wherein the swelling agent coating agent accounts for 5% of the swelling agent.

2. A composite top-jointing agent having both expansion and flow-promoting functions as claimed in claim 1, It is characterized in that The flow promoter is composed of 25-35% of powdered polycarboxylic acid water reducer, 0.5-2% of composite cellulose and 55-75% of sodium thiosulfate.

3. A composite top-jointing agent having both expansion and flow-promoting functions as claimed in claim 2, It is characterized in that The composite cellulose is prepared by mixing cellulose powders with a viscosity of 20000-50000 and 150000-200000 in a ratio of 7:

3.

4. A method for preparing a composite top-jointing agent having both expansion and flow-promoting functions as claimed in claim 1, It is characterized in that The expander and the expander coating agent are firstly mixed and ground at 70°C to form a modified expander. The expander coating agent will melt at 70°C. Through mixing and grinding, the coating agent forms an isolation film on the surface of the expander to delay the expansion time of the expander.

5. A method for preparing a composite top-jointing agent having both expansion and flow-promoting functions as claimed in claim 4, It is characterized in that The expansion component composed of the expansion agent and the expansion agent coating agent can be released after the concentrated expansion time is delayed by 1.0 hour.

6. A method for preparing a composite top-jointing agent having both expansion and flow-promoting functions as claimed in claim 1, It is characterized in that The flow promoter sustained-release agent can gradually release the water-reducing effect and extend the working time of the filling material by more than 1 hour.

7. A composite top-jointing agent having both expansion and flow-promoting functions as claimed in claim 1, It is characterized in that The top bonding agent is used to cement the coal gangue filling material, and the dosage is 2.0-6.0kg / m 3 , accounting for 0.1-0.3% of the total mass of the filling material, and the expansion rate can be adjusted within the range of 5%-15%.

8. A device for adding the composite capping agent with both expansion and flow-promoting functions as claimed in claims 1 to 7 to a cemented gangue filling material preparation system, It is characterized in that The machine comprises a frame, which is composed of an upper frame and a lower frame, wherein the upper frame is provided with a combination of a motor and a reducer, and a storage tank is provided at the lower part of the reducer, and the two are connected by a first connecting pipe; A metering tank is provided in the lower frame, and the storage tank and the metering tank are connected via a second connecting pipe; a stirring tank is provided at the lower part of the metering tank, and the metering tank and the stirring tank are connected via a third connecting pipe; and a water inlet valve is provided on the outer side of the stirring tank.