Near-all solid waste anti-rutting pavement material and construction method thereof

By using rut-resistant pavement materials composed of almost all solid waste, combined with cold-added asphalt and solid waste-based gelling materials, the problems of high maintenance costs and unenvironmental protection of existing pavement materials are solved, and efficient rut-resistant performance and Dynamic stability and energy-saving and environmentally friendly.

CN118908629APending Publication Date: 2024-11-08NANJING XINGYOU TRANSPORTATION TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410963913.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing pavement materials are costly and not environmentally friendly when facing rut diseases, and lack energy-saving and environmentally friendly materials that can effectively solve this problem.

Method used

Using rut-resistant pavement materials composed almost entirely of solid waste, including large gap asphalt mixture and grouting materials poured into it, improve the mechanical properties of the pavement through cold-added asphalt and solid waste-based gelling materials, and discard the grease through kitchen waste React with calcium carbide slag, white mud, etc. to achieve rapid grouting.

Benefits of technology

The water damage resistance and rut resistance of the road surface are significantly improved, and the dynamic stability is about 3-5 times that of conventional asphalt pavement, while achieving energy-saving and environmental protection of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention discloses a nearly all solid waste anti-rutting pavement material and a construction method thereof, the pavement material comprises a macrovoid asphalt mixture and a grouting material, the macrovoid asphalt mixture comprises an asphalt pavement reclaimed material and cold patch asphalt, and the cold patch asphalt comprises matrix asphalt, kitchen waste grease and triethanolamine; the grouting material comprises a solid waste-based cementing material, tailing sand, sodium sulfate, carbon black and the balance of water, wherein the solid waste-based cementing material comprises steel slag, red mud, water granulated slag, carbide slag and white mud; during construction, the large-gap asphalt mixture is firstly paved, then the grouting material is poured into the large-gap asphalt mixture, surface laitance is scraped off to form a structural joint, and maintenance is performed until traffic is opened. According to the pavement material disclosed by the invention, the inorganic slurry is poured into the large gaps, so that the asphalt mixture is wrapped by the slurry, the water damage resistance of the asphalt mixture is improved, meanwhile, the rutting resistance of the pavement is improved due to the high strength of the slurry, and the pavement material is almost completely composed of solid wastes and is energy-saving and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of pavement materials, and in particular relates to a nearly all-solid waste anti-rutting pavement material and a construction method thereof. Background Art

[0002] Rutting is one of the typical diseases of asphalt pavement. Frequent maintenance takes up a lot of maintenance funds and affects traffic. Semi-flexible pavement is a composite pavement technology formed by pouring high-flow cement-based materials into large-pore asphalt pavement. It can effectively cure rutting diseases and has been applied in many harsh rutting sections such as intersections, bus stations, BRT lanes, etc., and its application prospects are very broad.

[0003] Based on this, there is an urgent need for a new type of pavement material that can be composed almost entirely of solid waste, which not only has excellent pavement mechanical properties but is also energy-saving and environmentally friendly. Summary of the invention

[0004] Purpose of the invention: The present invention provides a new type of anti-rutting pavement material, which is almost entirely composed of solid waste, is energy-saving and environmentally friendly, and has excellent mechanical properties.

[0005] Technical solution: The nearly all-solid waste anti-rutting pavement material of the present invention comprises a large-void asphalt mixture and a grouting material poured into the large-void asphalt mixture;

[0006] The large-void asphalt mixture comprises, by mass fraction, 95-97% of asphalt pavement recycled material and 3-5% of cold patch asphalt; the cold patch asphalt comprises, by mass fraction, 70-73% of base asphalt, 20-25% of waste cooking oil and 4-7% of triethanolamine;

[0007] The grouting material includes, by mass fraction, 52-58% of solid waste-based cementitious material, 18-23% of tailings sand, 1.5-2% of sodium sulfate, 0.2-0.3% of carbon black and the balance of water; the solid waste-based cementitious material includes, by mass fraction, 30-35% of steel slag, 5-8% of red mud, 40-50% of water slag, 8-12% of carbide slag and 2-10% of white mud.

[0008] The present invention adopts rutting-resistant pavement materials which are almost entirely composed of solid waste, and cold patch asphalt is composed of base asphalt, waste kitchen grease and triethanolamine, and the cementitious material of the grouting material is composed of steel slag, red mud, slag, carbide slag and white mud. The cold patch asphalt has a long storage standby time, which can provide sufficient mixing time for the diffusion between new and old asphalt, that is, sufficient time for the function of the old asphalt to recover; and the triethanolamine in the cold patch asphalt can react with compounds such as carboxylic acids and epoxy compounds in the asphalt to generate corresponding salts or esters, so that the gel quality of the asphalt is reduced, and it is beneficial to enhance the adhesion between the asphalt and the aggregate; in addition, waste kitchen grease is used as a diluent in the cold patch asphalt, and the waste kitchen grease reacts with alkaline substances such as carbide slag, white mud and hydration products in the solid waste-based cementitious material to achieve the purpose of removal, so as to achieve rapid grouting, no volatilization, and environmental protection.

[0009] Furthermore, the volume fraction of the large-void asphalt mixture used in the pavement material is 75-85%, and the volume fraction of the grouting material is 15-25%.

[0010] Furthermore, the void ratio of the large-void asphalt mixture used in the pavement material is 18-27%.

[0011] Furthermore, the asphalt pavement recycled materials used in the pavement material are recycled materials after fine separation, of which 10-15mm recycled materials account for 8-10%, 5-10mm recycled materials account for 60-75%, 3-5mm recycled materials account for 5-10%, and 0-3mm recycled materials account for 11-20%.

[0012] Furthermore, the specific surface area of ​​steel slag, red mud, water slag, carbide slag and white mud used in the pavement materials is ≥400kg / m 2 The particle size of tailings sand is 40-70 mesh.

[0013] Furthermore, the cold patch asphalt used in the pavement material is prepared by the following steps: adding kitchen waste grease and triethanolamine into a base asphalt at 110-130° C., and stirring and mixing evenly.

[0014] Furthermore, the grouting material used in the pavement material is prepared by the following steps:

[0015] (1) Preparing a solid waste-based cementitious material: uniformly mixing steel slag, red mud, water slag, carbide slag and white mud to prepare a solid waste-based cementitious material;

[0016] (2) Preparation of grouting material: after the solid waste-based cementitious material is evenly mixed with tailings sand, sodium sulfate and carbon black, water is added and stirred to obtain the grouting material.

[0017] The construction method of the nearly all-solid waste anti-rutting pavement material of the present invention comprises the following steps:

[0018] (1) Paving large-void asphalt mixture: After the asphalt pavement recycled material and cold patch asphalt are evenly mixed, the large-void asphalt mixture is spread on the pavement base or the middle and lower layers, and rolled to make it dense;

[0019] (2) Pour grouting material into the large-void asphalt mixture, scrape off the surface slurry to form a structural joint, and maintain it until it is open to traffic.

[0020] Furthermore, in the construction method of the present invention, the paving thickness of the large-void asphalt mixture is 6-10 cm.

[0021] Beneficial effects: Compared with the prior art, the significant advantages of the present invention are: the pavement material improves the water damage resistance of the asphalt mixture by pouring inorganic slurry into large gaps, so that the asphalt mixture is wrapped by the slurry. At the same time, the high strength of the slurry improves the rutting resistance of the pavement, and its dynamic stability is about 3-5 times that of conventional asphalt pavement. The anti-rutting pavement material provided by the present invention is almost entirely composed of solid waste, which is energy-saving and environmentally friendly. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is further described in detail below in conjunction with embodiments.

[0023] It should be noted that the waste cooking oil used in the present invention comes from Hunan Renhe Environmental Protection Co., Ltd., steel slag comes from Nanjing Iron and Steel Group Co., Ltd., red mud comes from Shandong Xinfa Alumina Plant, water slag comes from Nanjing Iron and Steel Group Co., Ltd., calcium carbide slag comes from Shaanxi Beiyuan Chemical Group Co., Ltd., and white mud comes from Xuzhou Tianyuan Paper Co., Ltd. The composition of each substance is shown in Tables 1 and 2 below.

[0024] Table 1 Physical and chemical properties of waste cooking oil

[0025]

[0026] Table 2 Chemical composition of raw materials

[0027]

[0028] Example 1

[0029] The pavement material of this embodiment 1 includes 80% of large void asphalt mixture and 20% of grouting material by volume. The component contents of the large void asphalt mixture and the grouting material are shown in Table 3 and Table 4 below, respectively.

[0030] Table 3 Component contents of large void asphalt mixture of Example 1

[0031]

[0032]

[0033] Table 4 Component contents of the grouting material of Example 1

[0034]

[0035] The construction method of the pavement material of the embodiment 1 comprises the following steps:

[0036] (1) Adding waste cooking oil and triethanolamine into base asphalt at 120°C and mixing them evenly by mechanical stirring;

[0037] (2) adding recycled asphalt pavement material and mixing it evenly with the material in step (1), and after cooling to room temperature, sealing and storing it to obtain a large-void asphalt mixture;

[0038] (3) Spreading the large-void asphalt mixture prepared in (2) on the road base or the middle and lower layers, and rolling it to make it dense, with a paving thickness of 8 cm;

[0039] (4) Steel slag, red mud, water slag, carbide slag and white mud are mixed evenly to obtain a solid waste-based cementitious material; after the solid waste-based cementitious material is mixed evenly with tailings sand, sodium sulfate and carbon black, water is added and stirred to obtain a grouting material.

[0040] (5) After the asphalt mixture has formed strength, a grouting material is prepared according to the proportion and poured into the large-void asphalt mixture;

[0041] (6) Use a wool mop or rubber mop to push the slurry back and forth to scrape off the surface slurry to form a structural joint, and then maintain it until it is open to traffic.

[0042] Example 2

[0043] The pavement material of Example 2 includes a large void asphalt mixture with a volume fraction of 78% and a grouting material with a volume fraction of 22%. The component contents of the large void asphalt mixture and the grouting material are shown in Table 5 and Table 6 below, respectively.

[0044] Table 5 Component contents of large void asphalt mixture of Example 2

[0045]

[0046] Table 6 Component content of the grouting material of Example 2

[0047]

[0048] The construction method of the pavement material of this embodiment 2 is the same as that of embodiment 1.

[0049] Example 3

[0050] The pavement material of this embodiment 3 includes a large void asphalt mixture with a volume fraction of 75% and a grouting material with a volume fraction of 25%. The component contents of the large void asphalt mixture and the grouting material are shown in Table 7 and Table 8 below, respectively.

[0051] Table 7 Component contents of large void asphalt mixture of Example 3

[0052]

[0053] Table 8 Component content of the grouting material of Example 3

[0054]

[0055] The construction method of the pavement material of the third embodiment comprises the following steps:

[0056] (1) Adding waste cooking oil and triethanolamine into base asphalt at 110°C and mixing them evenly by mechanical stirring;

[0057] (2) adding recycled asphalt pavement material and mixing it evenly with the material in step (1), and after cooling to room temperature, sealing and storing it to obtain a large-void asphalt mixture;

[0058] (3) Spreading the large-void asphalt mixture prepared in (2) on the road base or the middle and lower layers, and rolling it to make it dense, with a paving thickness of 6 cm;

[0059] (4) Steel slag, red mud, water slag, carbide slag and white mud are mixed evenly to obtain a solid waste-based cementitious material; after the solid waste-based cementitious material is mixed evenly with tailings sand, sodium sulfate and carbon black, water is added and stirred to obtain a grouting material.

[0060] (5) After the asphalt mixture has formed strength, a grouting material is prepared according to the proportion and poured into the large-void asphalt mixture;

[0061] (6) Use a wool mop or rubber mop to push the slurry back and forth to scrape off the surface slurry to form a structural joint, and then maintain it until it is open to traffic.

[0062] Example 4

[0063] The pavement material of Example 4 includes 85% of large void asphalt mixture and 15% of grouting material by volume. The component contents of the large void asphalt mixture and the grouting material are shown in Tables 9 and 10 below, respectively.

[0064] Table 9 Component contents of large void asphalt mixture of Example 4

[0065]

[0066] Table 10 Component contents of the grouting material of Example 4

[0067]

[0068]

[0069] The construction method of the pavement material of the fourth embodiment comprises the following steps:

[0070] (1) Adding waste cooking oil and triethanolamine into base asphalt at 130°C and mixing them evenly by mechanical stirring;

[0071] (2) adding recycled asphalt pavement material and mixing it evenly with the material in step (1), and after cooling to room temperature, sealing and storing it to obtain a large-void asphalt mixture;

[0072] (3) Spreading the large-void asphalt mixture prepared in (2) on the road base or the middle and lower layers, and rolling it to make it dense, with a paving thickness of 10 cm;

[0073] (4) Steel slag, red mud, water slag, carbide slag and white mud are mixed evenly to obtain a solid waste-based cementitious material; after the solid waste-based cementitious material is mixed evenly with tailings sand, sodium sulfate and carbon black, water is added and stirred to obtain a grouting material.

[0074] (5) After the asphalt mixture has formed strength, a grouting material is prepared according to the proportion and poured into the large-void asphalt mixture;

[0075] (6) Use a wool mop or rubber mop to push the slurry back and forth to scrape off the surface slurry to form a structural joint, and then maintain it until it is open to traffic.

[0076] Comparative Example

[0077] The basic steps are the same as those in Example 1, except that diesel is used in the cold patch asphalt instead of waste cooking oil. The component contents are shown in Tables 11 and 12 below.

[0078] Table 11 Component content of large void asphalt mixture of comparative example

[0079]

[0080]

[0081] Table 12 Component content of the grouting material of the comparative example

[0082]

[0083] The pavement materials of the above-mentioned Examples 1-4 and the comparative example were prepared into anti-rutting specimens and subjected to performance testing. The results obtained are shown in Table 13 below.

[0084] Table 13 Performance test of samples of Examples 1-4 and Comparative Examples

[0085]

[0086]

[0087] It can be seen from Table 13 that the present invention adopts cold patch asphalt composed of base asphalt, waste cooking oil and triethanolamine, and the cementitious material of the grouting material composed of steel slag, red mud, slag, carbide slag and white mud. In the combination of the two, the waste cooking oil as a diluent is removed by reacting with alkaline substances such as carbide slag, white mud and hydration products in the solid waste-based cementitious material, thereby avoiding the diluent from being removed by volatilization and effectively reducing the grouting time of the grouting material, so as to achieve the purpose of grouting after the large-void asphalt mixture is compacted.

Claims

1. A nearly all-solid waste anti-rutting pavement material, characterized in that: The pavement material comprises a large-void asphalt mixture and a grouting material poured into the large-void asphalt mixture; The large-void asphalt mixture comprises, by mass fraction, 95-97% of asphalt pavement recycled material and 3-5% of cold patch asphalt; the cold patch asphalt comprises, by mass fraction, 70-73% of base asphalt, 20-25% of waste cooking oil and 4-7% of triethanolamine; The grouting material includes, by mass fraction, 52-58% of solid waste-based cementitious material, 18-23% of tailings sand, 1.5-2% of sodium sulfate, 0.2-0.3% of carbon black and the balance of water; the solid waste-based cementitious material includes, by mass fraction, 30-35% of steel slag, 5-8% of red mud, 40-50% of water slag, 8-12% of carbide slag and 2-10% of white mud.

2. The nearly all-solid waste anti-rutting pavement material according to claim 1, characterized in that: The volume fraction of the large-void asphalt mixture is 75-85%, and the volume fraction of the grouting material is 15-25%.

3. The nearly all-solid waste anti-rutting pavement material according to claim 1 or 2, characterized in that: The void ratio of the large-void asphalt mixture is 18-27%.

4. The nearly all-solid waste anti-rutting pavement material according to claim 1, characterized in that: The asphalt pavement recycled materials are recycled materials after fine separation, of which 10-15mm recycled materials account for 8-10%, 5-10mm recycled materials account for 60-75%, 3-5mm recycled materials account for 5-10%, and 0-3mm recycled materials account for 11-20%.

5. The nearly all-solid waste anti-rutting pavement material according to claim 1, characterized in that: The specific surface area of ​​the steel slag, red mud, water slag, carbide slag and white mud is ≥400kg / m 2 The particle size of tailings sand is 40-70 mesh.

6. The nearly solid waste anti-rutting pavement material according to claim 1, characterized in that: The cold patch asphalt is prepared by the following steps: adding waste cooking oil and triethanolamine into base asphalt at 110-130° C., and stirring and mixing evenly.

7. The nearly all-solid waste anti-rutting pavement material according to claim 1, characterized in that: The grouting material is prepared by the following steps: (1) Preparing a solid waste-based cementitious material: uniformly mixing steel slag, red mud, water slag, carbide slag and white mud to prepare a solid waste-based cementitious material; (2) Preparation of grouting material: after the solid waste-based cementitious material is evenly mixed with tailings sand, sodium sulfate and carbon black, water is added and stirred to obtain the grouting material.

8. The construction method of the nearly all-solid waste anti-rutting pavement material according to claim 1, characterized in that The steps include: (1) Paving large-void asphalt mixture: After the asphalt pavement recycled material and cold patch asphalt are evenly mixed, the large-void asphalt mixture is spread on the pavement base or the middle and lower layers, and rolled to make it dense; (2) Pour grouting material into the large-void asphalt mixture, scrape off the surface slurry to form a structural joint, and maintain it until it is open to traffic.

9. The construction method of the nearly all-solid waste anti-rutting pavement material according to claim 8, characterized in that: The paving thickness of the large-void asphalt mixture is 6-10 cm.