Method for industrial utilization of muck

Through separation, crushing and pulping of residues, fluid soil is prepared, which solves the problems of unsolid and low strength of residues, and achieves efficient and low cost utilization of residues, and meets the backfill strength requirements of various scenarios.

CN118908661APending Publication Date: 2024-11-08SHANGHAI SHENJI TRANSPORTATION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411026331.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing slag utilization methods have problems such as untightened backfill, low strength and high cost, and it is difficult to meet the requirements of high strength and anti-seepage.

Method used

Sludge and inorganic blocks are obtained by separating the slag, crushing them to obtain machine sand and steel bar blocks, removing organic matter and slurry, mixing cement, machine sand and slurry to prepare fluid soil, meeting the backfill requirements of different scenarios.

Benefits of technology

It realizes efficient utilization of slag, achieving backfilling strength requirements of 1 to 1.5MPa and 2 to 5MPa, which is simple to operate and low cost, and is suitable for a variety of scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908661A_ABST
    Figure CN118908661A_ABST
Patent Text Reader

Abstract

The invention provides a method for industrial utilization of muck, and belongs to the technical field of solid waste reutilization. The method provided by the invention comprises the following steps: separating the muck to obtain slurry and inorganic blocks; the inorganic blocks are crushed, and machine-made sand and reinforcing steel bar blocks are obtained through separation; removing organic matters from the slurry, and pulping to obtain slurry; cement, the machine-made sand and the slurry are mixed, and the fluid soil is obtained. According to the method, soil and inorganic blocks in the muck are separated, the inorganic blocks are crushed to prepare machine-made sand, and steel bar blocks are separated out and recycled; the slurry obtained by pulping the soil is mixed with the machine-made sand and the cement, so that the fluid soil meeting the requirements of different scenes can be obtained. The method provided by the invention is simple to operate and low in cost, and the muck can be efficiently utilized. The result of the embodiment shows that the fluid soil obtained by industrially utilizing the muck by adopting the method provided by the invention can meet the backfilling requirements of 1-1.5 MPa and 2-5 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste recycling, and in particular to a method for industrialized utilization of slag. Background Art

[0002] Muck is a type of construction waste, and its main components include soil, inorganic lumps and organic lumps. Among them, inorganic lumps include concrete blocks, bricks, glass, ceramics and steel bars; organic lumps include films, foams and wood. The composition of slag is relatively complex, which makes it difficult to comprehensively utilize it. It is generally utilized by backfilling foundation pits. However, when slag is backfilled, there are problems such as loose backfill, especially in narrow spaces where machinery cannot roll it or it is not compacted.

[0003] In the prior art, slag can be added to cement to form recycled materials, which can then be backfilled for use. However, due to the complex composition of slag, if it is directly backfilled in the above manner, the anti-seepage ability and strength after solidification are low, and it cannot meet the requirements of places with high strength requirements. Therefore, although the existing method can consume part of the slag, such a treatment method can only be used in places with low anti-seepage requirements and strength requirements, and its application is severely limited, and the slag cannot be used efficiently. In addition, in some construction sites, there will be excess slag backfilled in the above method, and it needs to be transported to other construction sites, resulting in high slag treatment costs.

[0004] Therefore, there is an urgent need to provide a method that is low in cost and can efficiently utilize slag. Summary of the invention

[0005] The object of the present invention is to provide a method which is low in cost and can efficiently utilize slag.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for industrial utilization of slag, comprising the following steps:

[0008] (1) Separating the slag into mud and inorganic blocks;

[0009] (2) crushing the inorganic blocks obtained in step (1) to obtain machine-made sand and steel blocks through separation;

[0010] (3) removing organic matter from the mud obtained in step (1), and then pulping to obtain slurry;

[0011] (4) mixing cement, the machine-made sand obtained in step (2) and the slurry obtained in step (3) to obtain fluidized soil;

[0012] There is no chronological order for steps (2) and (3).

[0013] Preferably, the separation method in step (1) comprises:

[0014] a. Use a separator to separate the soil and inorganic blocks in the slag to obtain soil and coarse inorganic blocks;

[0015] b. Use a high-pressure water gun to wash the coarse inorganic blocks obtained in step a to obtain inorganic blocks and muddy water, and mix the muddy water with the soil obtained in step a to obtain mud.

[0016] Preferably, the particle size of the machine-made sand in step (2) is less than 2 cm.

[0017] Preferably, the separation method in step (2) is magnetic separation.

[0018] Preferably, the specific gravity of the slurry in step (3) is 1.2 to 1.5 t / m 3 .

[0019] Preferably, the specific gravity of the slurry is 1.2-1.3 t / m 3 or 1.3~1.5t / m 3 .

[0020] Preferably, the specific gravity of cement in the fluidized soil in step (4) is 60-135 kg / m 3 .

[0021] Preferably, the specific gravity of cement in the fluidized soil is 60-91 kg / m 3 Or 90~135Kg / m 3 .

[0022] Preferably, the specific gravity of the machine-made sand in the fluidized soil in step (4) is 0 to 700 kg / m 3 .

[0023] Preferably, the specific gravity of the machine-made sand in the fluidized soil is 200-700 Kg / m 3 .

[0024] The present invention provides a method for industrial utilization of slag, comprising the following steps: separating the slag to obtain mud and inorganic blocks; crushing the inorganic blocks to obtain machine-made sand and steel blocks through separation; removing organic matter from the slurry, pulping to obtain slurry; mixing cement, the machine-made sand and the slurry to obtain fluidized soil. The present invention separates the mud and inorganic blocks in the slag, prepares the inorganic blocks into machine-made sand by crushing, and separates the steel blocks for recycling; the present invention pulps the mud, mixes the obtained slurry with machine-made sand and cement, and can obtain fluidized soil that meets the requirements of different scenarios. In addition, the method provided by the present invention is simple to operate, low in cost, and can efficiently utilize the slag. The results of the embodiment show that the fluidized soil obtained by industrially utilizing the slag using the method provided by the present invention can meet the backfill requirements of 1 to 1.5 MPa and 2 to 5 MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A schematic diagram of the method for industrial utilization of slag provided by the present invention;

[0026] Figure 2 A schematic diagram of preparing machine-made sand using inorganic blocks in the method for industrial utilization of slag provided by the present invention;

[0027] Figure 3 A schematic diagram of preparing fluidized soil in the method for industrial utilization of slag provided by the present invention;

[0028] Figure 4 A schematic diagram of the fluidized soil prepared in Example 1 of the present invention being used for backfilling a foundation pit;

[0029] Figure 5 A schematic diagram of the fluidized soil prepared in Example 2 of the present invention being used for pipeline protection;

[0030] Figure 6 This is a schematic diagram of the fluidized soil prepared in Examples 3 to 4 of the present invention being used for road foundation. DETAILED DESCRIPTION

[0031] The present invention provides a method for industrial utilization of slag, comprising the following steps:

[0032] (1) Separating the slag into mud and inorganic blocks;

[0033] (2) crushing the inorganic blocks obtained in step (1) to obtain machine-made sand and steel blocks through separation;

[0034] (3) removing organic matter from the mud obtained in step (1), and then pulping to obtain slurry;

[0035] (4) mixing cement, the machine-made sand obtained in step (2) and the slurry obtained in step (3) to obtain fluidized soil;

[0036] There is no chronological order for steps (2) and (3).

[0037] The present invention separates the slag into mud and inorganic blocks;

[0038] In the present invention, the separation method preferably comprises:

[0039] a. Use a separator to separate the soil and inorganic blocks in the slag to obtain soil and coarse inorganic blocks;

[0040] b. Use a high-pressure water gun to wash the coarse inorganic blocks obtained in step a to obtain inorganic blocks and muddy water, and mix the muddy water with the soil obtained in step a to obtain mud.

[0041] The present invention preferably uses a separator to separate the soil and inorganic blocks in the slag to obtain soil and coarse inorganic blocks.

[0042] In the present invention, the separator is preferably a roller separator. The present invention uses a roller separator to separate the slag, and the ribs on the roller can decompose the soil when rolling, and the inorganic matter and soil smaller than 2 cm are sieved from the gap of the roller through vibration; at the same time, the inorganic hard blocks larger than 2 cm are transported forward by the ribbed roller, so as to achieve the separation of soil and inorganic blocks.

[0043] After obtaining the mud and the roughly divided inorganic blocks, the present invention preferably uses a high-pressure water gun to wash the roughly divided inorganic blocks to obtain inorganic blocks and muddy water, and the muddy water is mixed with the mud to obtain mud. The present invention uses the impact force of the high-pressure water gun to fully separate the mud stuck in the inorganic blocks, and the obtained muddy water is mixed with the mud separated by the separator to obtain mud. The present invention does not specifically limit the model and parameters of the high-pressure water gun, and a commonly used high-pressure water gun can be used to fully separate the mud and the inorganic blocks.

[0044] After obtaining the inorganic blocks, the present invention crushes the inorganic blocks to obtain machine-made sand and steel bars through separation.

[0045] The present invention has no special limitation on the crushing method. A conventional crushing method can be used to make the size of the machine-made sand reach the required size. In the present invention, the device used for crushing is preferably a crusher. In the present invention, the particle size of the machine-made sand is preferably less than 2 cm.

[0046] In the present invention, the separation method is preferably magnetic separation. The present invention separates the machine-made sand from the steel bar blocks by separation, the steel bar blocks can be recycled, and the machine-made sand is used to prepare fluidized soil. The present invention has no special limitation on the operation method of the magnetic separation, and a conventional magnetic separation operation method is used to fully separate the steel bar blocks from the crushed particles.

[0047] In the present invention, the inorganic blocks are preferably crushed and then the organic matter is separated by screening. The present invention has no particular limitation on the screening method, as long as the organic matter in the crushed particles can be fully removed.

[0048] After obtaining the mud, the present invention removes organic matter from the mud and then performs pulping to obtain slurry.

[0049] The present invention has no special limitation on the method of removing organic matter from the mud, and conventional methods can be used to fully separate the organic matter from the mud. In the present invention, since the density of organic matter is relatively low and it is distributed on the surface of the mud, the present invention salvages the organic matter on the surface of the mud.

[0050] In the present invention, the slurry making method preferably comprises: removing organic matter from the slurry, allowing the slurry to stand and solidify, and then mixing the solidified slurry with water to obtain slurry.

[0051] The present invention does not specifically limit the amount of water used, and it can be adjusted according to the amount of solidified mud used to make the specific gravity of the slurry reach the required value. In the present invention, the specific gravity of the slurry is preferably 1.2 to 1.5 t / m 3 , more preferably 1.2 to 1.3 t / m 3 or 1.3~1.5t / m 3 The present invention controls the specific gravity of the slurry within the above range and can be used in combination with other components to achieve the fluidized soil required for backfill strength.

[0052] After obtaining the machine-made sand and the slurry, the present invention mixes cement, the machine-made sand and the slurry to obtain fluidized soil.

[0053] In the present invention, the cement dosage is 60-135 kg / m 3 , more preferably 60 to 91 kg / m 3 Or 90~135Kg / m 3 The amount of cement used is 60-91 kg / m 3 The dosage is preferably 5-7%, and the dosage of the cement is 90-135 Kg / m 3 In the present invention, the specific gravity of the machine-made sand in the fluidized soil is preferably 0-700 Kg / m 3 , more preferably 200 to 700 Kg / m 3 The present invention controls the specific gravity of the machine-made sand in the cement and fluidized soil within the above range, and can be used in combination with the slurry to achieve the required backfill strength of the fluidized soil. In the present invention, the specific gravity of the slurry in the fluidized soil is 1.2-1.3 t / m 3 The specific gravity of cement in fluidized soil is 60~91Kg / m 3When the fluidized soil is obtained, the backfill requirement is 1-1.5 MPa; the specific gravity of the slurry in the fluidized soil is 1.3-1.5 t / m 3 The specific gravity of cement in fluidized soil is 91~135Kg / m 3 The specific gravity of machine-made sand in fluidized soil is 200~700Kg / m 3 The fluidized soil obtained can meet the backfill requirements of 1.5~5MPa.

[0054] The present invention has no special limitation on the method for mixing the cement, the machine-made sand and the slurry. A conventional mixing method can be used to obtain fluidized soil.

[0055] The schematic diagram of the method for industrial utilization of slag provided by the present invention is preferably as follows Figure 1 As shown. Figure 1 In the present invention, the slag is first passed through a separator to obtain inorganic blocks and mud, and the inorganic blocks are crushed to obtain machine-made sand; the mud is removed of organic matter and then enters a mud pool.

[0056] The schematic diagram of using inorganic blocks to prepare machine-made sand in the method for industrial utilization of slag provided by the present invention is preferably as follows: Figure 2 As shown. Figure 2 In the present invention, the inorganic blocks are crushed to recover the steel bars and remove the organic matter, so that the particles smaller than 2 cm are obtained as machine-made sand, and the broken pieces larger than 2 cm are returned to the crusher for crushing to obtain machine-made sand.

[0057] The schematic diagram of preparing fluidized soil in the method for industrial utilization of slag provided by the present invention is preferably as follows Figure 3 As shown. Figure 3 In the present invention, the mud is slurried, and then mixed with machine-made sand and cement to obtain fluidized soil for application.

[0058] The method provided by the present invention is simple to operate, can recycle steel bars in slag, and can prepare fluidized soil that meets various backfill requirements from mud and machine-made sand, thereby achieving efficient utilization of slag.

[0059] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0060] Example 1

[0061] A method for industrial utilization of slag, comprising the following steps:

[0062] (1) The slag is separated by a roller-type separator, and the ribs on the roller are used to decompose the soil. The inorganic matter and soil smaller than 2 cm are sieved out from the gaps of the roller by vibration. At the same time, the inorganic blocks larger than 2 cm are transported forward by the ribbed roller. The inorganic blocks are then washed with a high-pressure water gun to obtain inorganic blocks, and the mud on the inorganic blocks is separated to obtain mud water, which is mixed with the soil to obtain mud;

[0063] (2) crushing the inorganic blocks obtained in step (1) with a crusher to reduce the particle size to less than 2 cm, and returning particles larger than 2 cm to the crusher for further crushing; separating particles with a particle size less than 2 cm by magnetic separation to obtain machine-made sand and steel blocks, and recycling the steel blocks;

[0064] (3) The organic matter on the surface of the mud obtained in step (1) is salvaged and removed, and then solidified in a mud pool to obtain solidified mud. The solidified mud is mixed with water to obtain slurry. The specific gravity of the slurry is 1.3 t / m 3 ;

[0065] (4) Add PO42.5 silicate cement (the specific gravity of cement in fluidized soil is 90Kg / m 3 ) and the slurry obtained in step (3) are made into a large-scale mixing and stirring equipment through a double-hinged cage method. The stirring equipment is equipped with an automatic weighing and distribution system. According to the requirements of the mix ratio, various raw materials for generating fluidized soil are automatically added, and the materials are automatically fed and stirred to generate fluidized soil that meets the requirements of the mix ratio.

[0066] The fluidized soil prepared in this embodiment is used for foundation pit backfilling. The backfilling requirements are: the strength of the fluidized soil is 1-1.5MPa. The pit backfilling can be poured in one time. The fluidized soil will be self-compacting and has a good waterproofing function for the wall. Figure 4 shown.

[0067] Example 2

[0068] A method for industrial utilization of slag, comprising the following steps:

[0069] (1) The slag is separated by a roller-type separator, and the ribs on the roller are used to decompose the soil. The inorganic matter and soil smaller than 2 cm are sieved out from the gaps of the roller by vibration. At the same time, the inorganic blocks larger than 2 cm are transported forward by the ribbed roller. The inorganic blocks are then washed with a high-pressure water gun to obtain inorganic blocks, and the mud on the inorganic blocks is separated to obtain mud water, which is mixed with the soil to obtain mud;

[0070] (2) crushing the inorganic blocks obtained in step (1) with a crusher to reduce the particle size to less than 2 cm, and returning particles larger than 2 cm to the crusher for further crushing; separating particles with a particle size less than 2 cm by magnetic separation to obtain machine-made sand and steel blocks, and recycling the steel blocks;

[0071] (3) The organic matter on the surface of the mud obtained in step (1) is salvaged and removed, and then solidified in a mud pool to obtain solidified mud. The solidified mud is mixed with water to obtain slurry. The specific gravity of the slurry is 1.4 t / m 3 ;

[0072] (4) Add PO42.5 silicate cement (the specific gravity of cement in fluidized soil is 130Kg / m 3 ), the machine-made sand obtained in step (2) (the specific gravity of the machine-made sand in the fluidized soil is 600Kg / m 3 ) and the slurry obtained in step (3) are made into a large-scale mixing and stirring equipment through a double-hinged cage method. The stirring equipment is equipped with an automatic weighing and distribution system. According to the requirements of the mix ratio, various raw materials for generating fluidized soil are automatically added, and the materials are automatically fed and stirred to generate fluidized soil that meets the requirements of the mix ratio.

[0073] The fluidized soil prepared in this embodiment is used for pipeline protection. The schematic diagram of pipeline protection is as shown in FIG. Figure 5 As shown, in Figure 5 The backfill requirements for the middle and lower parts of the fluidized soil are: the strength of the fluidized soil is 1~1.5MPa; the backfill requirements for the upper part of the fluidized soil are: the strength of the fluidized soil is 1.5~5MPa.

[0074] When fluidized soil is used for pipeline protection, the construction of the upper and lower structural layers should be divided into two operations. The lower part uses the fluidized soil prepared in Example 1, and the upper part uses the fluidized soil prepared in Example 2.

[0075] Example 3

[0076] A method for industrial utilization of slag, comprising the following steps:

[0077] (1) The slag is separated by a roller-type separator, and the ribs on the roller are used to decompose the soil. The inorganic matter and soil smaller than 2 cm are sieved out from the gaps of the roller by vibration. At the same time, the inorganic blocks larger than 2 cm are transported forward by the ribbed roller. The inorganic blocks are then washed with a high-pressure water gun to obtain inorganic blocks, and the mud on the inorganic blocks is separated to obtain mud water, which is mixed with the soil to obtain mud;

[0078] (2) crushing the inorganic blocks obtained in step (1) with a crusher to reduce the particle size to less than 2 cm, and returning particles larger than 2 cm to the crusher for further crushing; separating particles with a particle size less than 2 cm by magnetic separation to obtain machine-made sand and steel blocks, and recycling the steel blocks;

[0079] (3) The organic matter on the surface of the mud obtained in step (1) is salvaged and removed, and then solidified in a mud pool to obtain solidified mud. The solidified mud is mixed with water to obtain slurry. The specific gravity of the slurry is 1.3 t / m3 ;

[0080] (4) Add PO42.5 silicate cement (the specific gravity of cement in fluidized soil is 90Kg / m 3 ) and the slurry obtained in step (3) are made into a large-scale mixing and stirring equipment through a double-hinged cage method. The stirring equipment is equipped with an automatic weighing and distribution system. According to the requirements of the mix ratio, various raw materials for generating fluidized soil are automatically added, and the materials are automatically fed and stirred to generate fluidized soil that meets the requirements of the mix ratio.

[0081] The fluidized soil prepared in this embodiment is used for the lower structure of the road foundation, and the strength requirement of the fluidized soil of the lower structure is 1 to 1.5 MPa.

[0082] Schematic diagram of road foundation Figure 6 shown.

[0083] Example 4

[0084] A method for industrial utilization of slag, comprising the following steps:

[0085] (1) The slag is separated by a roller-type separator, and the ribs on the roller are used to decompose the soil. The inorganic matter and soil smaller than 2 cm are sieved out from the gaps of the roller by vibration. At the same time, the inorganic blocks larger than 2 cm are transported forward by the ribbed roller. The inorganic blocks are then washed with a high-pressure water gun to obtain inorganic blocks, and the mud on the inorganic blocks is separated to obtain mud water, which is mixed with the soil to obtain mud;

[0086] (2) crushing the inorganic blocks obtained in step (1) with a crusher to reduce the particle size to less than 2 cm, and returning particles larger than 2 cm to the crusher for further crushing; separating particles with a particle size less than 2 cm by magnetic separation to obtain machine-made sand and steel blocks, and recycling the steel blocks;

[0087] (3) The organic matter on the surface of the mud obtained in step (1) is salvaged and removed, and then solidified in a mud pool to obtain solidified mud. The solidified mud is mixed with water to obtain slurry. The specific gravity of the slurry is 1.4 t / m 3 ;

[0088] (4) Add PO42.5 silicate cement (the specific gravity of cement in fluidized soil is 130Kg / m 3 ), the machine-made sand obtained in step (2) (the specific gravity of the machine-made sand in the fluidized soil is 600Kg / m 3 ) and the slurry obtained in step (3) are made into a large-scale mixing and stirring equipment through a double-hinged cage method. The stirring equipment is equipped with an automatic weighing and distribution system. According to the requirements of the mix ratio, various raw materials for generating fluidized soil are automatically added, and the materials are automatically fed and stirred to generate fluidized soil that meets the requirements of the mix ratio.

[0089] The fluidized soil prepared in this embodiment is used for the upper structure of the road foundation. The strength requirement of the fluidized soil of the upper structure is 1.5-5 MPa. The schematic diagram of the road foundation is as follows Figure 6 As shown. The lower structure layer can be poured in place at one time. When the lower structure layer has reached a certain strength, the upper structure can be constructed immediately. When the strength of the upper structure layer reaches the design requirements, the asphalt layer can be spread. The construction is fast and the cycle can be greatly shortened.

[0090] From the above results, it can be seen that the method provided by the present invention separates the soil and inorganic blocks in the slag, crushes the inorganic blocks to prepare machine-made sand, and separates the steel blocks for recycling; the soil is pulped, and the obtained slurry is mixed with machine-made sand and cement to obtain fluidized soil that meets the requirements of different scenarios. In addition, the method provided by the present invention is simple to operate, low in cost, and can efficiently utilize slag.

[0091] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for industrial utilization of slag, comprising the following steps: (1) Separating the slag into mud and inorganic blocks; (2) crushing the inorganic blocks obtained in step (1) to obtain machine-made sand and steel blocks through separation; (3) removing organic matter from the mud obtained in step (1), and then pulping to obtain slurry; (4) mixing cement, the machine-made sand obtained in step (2) and the slurry obtained in step (3) to obtain fluidized soil; There is no chronological order for steps (2) and (3).

2. The method for industrial utilization of slag according to claim 1, characterized in that: The separation method in step (1) comprises: a. Use a separator to separate the soil and inorganic blocks in the slag to obtain soil and coarse inorganic blocks; b. Use a high-pressure water gun to wash the coarse inorganic blocks obtained in step a to obtain inorganic blocks and muddy water, and mix the muddy water with the soil obtained in step a to obtain mud.

3. The method for industrial utilization of slag according to claim 1, characterized in that: The particle size of the machine-made sand in step (2) is less than 2 cm.

4. The method for industrial utilization of slag according to claim 1, characterized in that: The separation method in step (2) is magnetic separation.

5. The method for industrial utilization of slag according to claim 1, characterized in that: The specific gravity of the slurry in step (3) is 1.2 to 1.5 t / m 3 .

6. The method for industrial utilization of slag according to claim 5, characterized in that: The specific gravity of the slurry is 1.2-1.3 t / m 3 or 1.3~1.5t / m 3 .

7. The method for industrial utilization of slag according to claim 1, characterized in that: The specific gravity of cement in the fluidized soil of step (4) is 60-135 kg / m 3 .

8. The method for industrial utilization of slag according to claim 7, characterized in that: The specific gravity of cement in the fluidized soil is 60-91 kg / m 3 Or 90~135Kg / m 3 .

9. The method for industrial utilization of slag according to claim 1, characterized in that: The specific gravity of the machine-made sand in the fluidized soil of step (4) is 0-700 kg / m 3 .