Physical-chemical combined activation recycling method for regenerated micro powder
By combining high-efficiency ball milling in a liquid environment with chemical additives, the activity of regenerated micro powder is improved, solving the problems of low environmental efficiency and high energy consumption in the treatment of regenerated micro powder, and realizing the efficient utilization of regenerated micro powder in building materials.
Patent Information
- Application Number
- CN202411244979.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-08
AI Technical Summary
Existing technologies for processing recycled micropowder suffer from low environmental efficiency, high energy consumption, and limited activation effects, which restricts its efficient use in building materials.
By combining high ball milling efficiency in a liquid environment with chemical additives, the activity of regenerated micro powder is improved through wet milling and the addition of chemical additives with grinding aid and complexing effects, such as alkanolamines with hydroxyl, amino, and phosphate groups. Stable complexes are formed in the liquid phase, increasing the solubility of metal ions.
It significantly improves the activity of regenerated micro powder, with an activity index of up to 75%, reduces energy consumption, simplifies the process, and realizes the efficient resource utilization of regenerated micro powder, which is in line with the goal of low-carbon development.
Smart Images

Figure CN118908669A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a method for physical-chemical combined activation and regeneration of regenerated micropowder. Background Art
[0002] With the advancement of global industrialization and urbanization, the building area has steadily increased, leading to an increasing demand for concrete. However, every year, urban construction and demolition generate a large amount of waste concrete. Waste concrete is often directly transported to the suburbs, piled in the open air or landfilled, which not only causes environmental pollution but also causes huge economic losses. The main method of utilizing construction waste at home and abroad is to crush and grind it. Recycled aggregates treated by mechanical and chemical methods have been widely used in engineering projects. However, in the process of preparing recycled coarse aggregate and recycled fine aggregate, a large amount of recycled concrete powder with a particle size of less than 0.16 mm will inevitably be produced, accounting for 5% to 20% of the total crushed material. Faced with the high water absorption, diversified sources and complex composition of recycled concrete powder, its reuse process presents obvious challenges. The large porosity and water absorption of recycled micropowder may significantly affect the workability, physical and mechanical properties and durability of the material when it is used in building materials such as concrete.
[0003] Existing studies have shown that the chemical composition of recycled micropowder is mainly composed of CaO, SiO2 and Al2O3, which makes it have potential gelling activity. Therefore, as an auxiliary cementing material, construction solid waste powder has the potential to partially replace cement. As an auxiliary cementing material, partial replacement of cement can not only reduce cement and energy consumption, but also help improve the utilization rate of construction solid waste and environmental protection. Recycled micropowder activation methods can be divided into physical (mechanical) activation, chemical activation and thermal (high temperature) activation. Compared with chemical activation, physical activation and thermal activation can more effectively improve the reaction activity of recycled micropowder. However, when using activation methods such as heat treatment to stimulate the activity of recycled micropowder, on the one hand, the energy consumption is relatively high, and on the other hand, a large amount of CO2 will be generated during the treatment process, which is contrary to the country's advocacy of economy, environmental protection and low energy consumption.
[0004] Grinding is a process that uses mechanical force to refine regenerated micropowders to increase their activity. Dry grinding processes are usually used for regenerated micropowders. However, as the particle size decreases, the surface energy of the particles increases significantly, making the particles more likely to agglomerate, and the grinding energy consumption also surges accordingly, making it challenging to further reduce the fineness. Wet grinding using liquid media can reduce the surface energy of the material and prevent particle agglomeration. At the same time, adding chemical admixtures with grinding aids and complexing effects during ball milling can, on the one hand, significantly reduce particle agglomeration during the grinding process, improve grinding efficiency, and optimize particle size distribution; on the other hand, in the liquid environment, the hydroxyl, amine, and phosphate groups in the chemical admixtures react with the metal ions (Ca2+) of the micropowder in the liquid.2+ ) form complexes, improve ion dissolution and increase activity. In addition, during the cement hydration and hardening process, chemical admixtures can affect the cement's setting time, strength development and other properties by affecting the cement hydration process.
[0005] CN 106242336 A discloses a method for preparing building mortar using construction waste. The invention prepares construction waste powder by special processes such as screening, grinding, and homogenization, and prepares mortar by compounding. The specific operation of preparing construction waste powder by this invention method is not detailed enough, and the particle size of the construction waste powder prepared by this method is not fine enough, and the activity stimulation of the construction waste powder is limited, which limits its efficient use in building materials.
[0006] CN116283022 A discloses a carbonization reactivation method using construction waste micropowder. The invention adopts the method of making construction waste micropowder into a reinforced slurry and then air-drying it. On the one hand, no chemical active admixture is added, and the activation effect of the construction waste micropowder is limited. The preparation process is complicated by the need to introduce CO2. On the other hand, the slurry is not directly utilized after air-drying, which makes the process more complicated and the utilization of the construction waste micropowder is limited. Summary of the invention
[0007] In view of the large stock of recycled micropowder, the environmental pollution and low efficiency of the existing technology in processing recycled micropowder, the present invention provides a method for physical-chemical combined activation and regeneration of recycled micropowder. On the one hand, the method of the present invention alleviates the pollution and economic losses of recycled micropowder to the natural environment, and on the other hand, the partial replacement of recycled micropowder for cement alleviates the problems of carbon emission and energy consumption of cement, and provides a feasible solution for efficient resource utilization of recycled micropowder.
[0008] The present invention performs low-carbon treatment on the regenerated micropowder, utilizes the high ball milling efficiency and high dispersibility in the liquid environment, and utilizes the hydroxyl, amine and phosphate groups in the chemical additives to react with the metal ions (Ca) of the micropowder in the liquid. 2+ ) to form a complex, thereby improving the dissolution and activity of the metal ions in the powder. The present invention can significantly improve the regeneration of the powder Ca after the chemical admixture is combined with low carbon. 2+ It has good solubility and activity, with an activity of up to 75%; and after the combined treatment, the slurry can be directly formed without drying, the process is simple, and it is in line with the national low-carbon development goals.
[0009] The method for physical-chemical combined activation and regeneration of regenerated micropowder of the present invention comprises the following steps: Step 1: Collect the demolished construction waste and place it in a multi-stage crusher to obtain waste concrete recycled micro powder through crushing, screening and sorting; Step 2: Take 10-25 parts of waste concrete recycled micro powder and mix it with 10-45 parts of water, add 0.02-0.2 parts of chemical admixture, and wet-ball mill for 30 minutes to obtain recycled micro powder slurry; Step 3: Mix 10-30 parts of the regenerated micropowder slurry with 60-90 parts of cement and 5-40 parts of water, and then pour the obtained cement-micropowder slurry into a mold for molding, and obtain the cement-micropowder pure slurry material through vibration and curing.
[0010] The above-mentioned feed ratio is calculated by mass.
[0011] In step 1, the particle size of the waste concrete recycled fine powder is ≤0.16 mm.
[0012] In step 2, the chemical admixture is one or more of alcoholamines and phosphate group substances having hydroxyl, amine and phosphate groups with grinding aid and chemical complexing effects, specifically selected from one or more of triethanolamine and triisopropanolamine. Both are thick liquids and need to be placed in water and stirred until fully dispersed before use.
[0013] In step 2, during wet ball milling, the ball-to-material ratio in the ball mill is 1:1-3:1, the water-to-material ratio is 1:1-1:2, the grinding balls are made of zirconia and the grading is 18-22mm:9-11mm:3.5-4mm=3:6:1, and the ball mill speed is 400r / min.
[0014] In step 3, the cement is P·O 42.5 grade cement.
[0015] In step 3, the water-cement ratio is 0.4-0.5.
[0016] In step 3, the test block needs to be cured for 24 hours before demolding and for 28 days after demolding. The curing environment is 20±2℃ and the humidity is not less than 95%.
[0017] The regenerated micro powder slurry is a directly processable slurry composed of regenerated micro powder, water and chemical admixtures. The water required for preparing cement-micro powder slurry test blocks needs to be deducted from the water dosage in the slurry and added into the mixer.
[0018] The present invention adds activated regenerated micro-powder slurry into cement paste to replace 10%-40% of cement dosage, so that the activated regenerated micro-powder slurry can be widely used in cement-based materials.
[0019] After being treated by the method of the present invention, the solubility of metal ions in the solution increases continuously, and the metal ions are complexed with anions in the chemical auxiliary agent and continue to dissolve.
[0020] The technical principle of the present invention is: The collected regenerated micropowder is mixed with admixtures and wet-milled to prepare an active auxiliary cementitious material. First, the regenerated micropowder is subjected to mechanical ball milling, which can refine the particles and increase the surface activity. On the other hand, it can transform the existing crystalline ordered structure in the micropowder into an amorphous amorphous structure. At the same time, the unhydrated clinker encapsulated in the regenerated micropowder is released and can be rehydrated. In the wet-milling process, chemical additives with complexing effects are added. On the one hand, it can improve the ball milling efficiency and reduce energy consumption. On the other hand, it can react with metal ions (Ca 2+ Mg 2+ ) form a stable complex, and the alkaline environment makes it easier for ions in the solid to dissolve. Finally, the microcrystalline nuclei generated in the liquid phase can enhance the early hydration reaction and improve the stability and consistency of the cementitious material. In addition, since the slurry treated with chemical admixtures contains the liquid and slurry required for the slurry test block molding, it does not need to be dried and molded again, which can reduce the problems of complex preparation process, low economic benefits, and poor sustainable development capabilities in the existing technology.
[0021] The beneficial effects of the present invention are embodied in: (1) The present invention adds a grinding aid and chemical complexing agent during the wet grinding process to improve the grinding aid effect while increasing the dissolution of active ions, and controls the concentration of calcium ions through complexation to adjust the hydration reaction rate.
[0022] (2) The auxiliary cementitious material prepared by the low-carbon method of the present invention has an activity index of more than 65%, which can achieve high-value utilization of construction waste.
[0023] (3) Use chemical admixtures with wet grinding and modification effects. As grinding aids, they can reduce energy consumption and improve the particle size distribution and performance of powders. As performance modifiers, on the one hand, they interact with mineral phases in cement, such as C3A and C3S, to affect the hydration rate of cement and the formation of hydration products, thereby improving the early strength of cement and facilitating the early hardening process of cement paste; on the other hand, they can participate in the generation of certain hydration products with specific structures, improve the density and durability of the matrix, and improve the workability of concrete and paste by affecting the viscosity and fluidity of cement paste.
[0024] (4) The auxiliary cementitious material slurry prepared by this method has better grading and higher activity. It does not need to be dried after wet grinding and can be directly formed according to the proportion. The construction is convenient and fast, the energy consumption is significantly reduced, and it has good stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0026] Figure 1 The ion dissolution amount of the materials prepared in comparative examples and embodiments.
[0027] Figure 2 The setting time of the auxiliary gelling materials prepared in the comparative examples and the examples is controlled. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is further specifically described below through examples, but the described implementation manner is only a part of the implementation manner of the present invention, rather than all the implementation manners, and the implementation manner of the present invention is not limited thereto.
[0029] The cement used in the following examples is commercially available P·O 42.5 silicate cement, which meets the standard requirements of "General Portland Cement" (GB 175-2007). The chemical admixture is a commercially available triethanolamine grinding aid or triisopropanolamine grinding aid, analytically pure. The water is tap water. The construction waste is provided by a construction waste site in Anhui; the crushing, screening and sorting equipment is jointly developed by the cooperative units of our school, and the crusher includes a jaw crusher, an impact crusher, an impact crusher, etc. Embodiment 1:
[0030] The method for preparing high-activity regenerated micropowder by combining low carbon with each other in this embodiment comprises the following steps: (1) Wet-mill a mixture of 20 parts of recycled micro powder with a particle size less than 0.16 mm, 0.04 parts of triethanolamine and 15 parts of water for 30 minutes to obtain an active auxiliary gelling material slurry. The wet-milling conditions are: ball-to-material ratio of 1:2.5, water-to-material ratio of 3:4, grinding ball particle size and grading of 18-22 mm:9-11 mm:3.5-4 mm = 3:6:1, and the ball mill speed of 400 r / min.
[0031] (2) Take 27 parts of the micropowder slurry obtained in step (1), mix with 63 parts of cement and 16 parts of water, and obtain a cement-recycled micropowder sample after vibration, molding and curing. The curing conditions are: the temperature is 20±2°C and the humidity is not less than 95% within 28 days. Embodiment 2:
[0032] The method for preparing high-activity regenerated micropowder by combining low carbon with each other in this embodiment comprises the following steps: (1) Wet-mill a mixture of 20 parts of regenerated micropowder with a particle size less than 0.16 mm, 0.06 parts of triethanolamine and 15 parts of water for 30 minutes to obtain a regenerated micropowder slurry with a finer median particle size. The wet-milling conditions are: ball-to-material ratio of 1:2.5, water-to-material ratio of 3:4, grinding ball particle size and grading of 18-22 mm:9-11 mm:3.5-4 mm = 3:6:1, and the ball mill speed of 400 r / min.
[0033] (2) Take 27 parts of the micropowder slurry obtained in step (1), mix with 63 parts of cement and 16 parts of water, and obtain a cement-recycled micropowder sample after vibration, molding and curing. The curing conditions are: the temperature is 20±2°C and the humidity is not less than 95% within 28 days. Embodiment 3:
[0034] The method for physical-chemical combined activation and regeneration of regenerated micropowder in this embodiment comprises the following steps: (1) Wet-mill a mixture of 20 parts of regenerated micropowder with a particle size less than 0.16 mm, 0.08 parts of triethanolamine and 15 parts of water for 30 minutes to obtain a regenerated micropowder slurry with a finer median particle size. The wet-milling conditions are: ball-to-material ratio of 1:2.5, water-to-material ratio of 3:4, grinding ball particle size and grading of 18-22 mm:9-11 mm:3.5-4 mm = 3:6:1, and the ball mill speed of 400 r / min.
[0035] (2) Take 27 parts of the micropowder slurry obtained in step (1), mix with 63 parts of cement and 16 parts of water, and obtain a cement-recycled micropowder sample after vibration, molding and curing. The curing conditions are: the temperature is 20±2°C and the humidity is not less than 95% within 28 days. Embodiment 4:
[0036] The method for physical-chemical combined activation and regeneration of regenerated micropowder in this embodiment comprises the following steps: (1) Wet-mill a mixture of 20 parts of regenerated micropowder with a particle size less than 0.16 mm, 0.10 parts of triethanolamine and 15 parts of water for 30 minutes to obtain a regenerated micropowder slurry with a finer median particle size. The wet-milling conditions are: ball-to-material ratio of 1:2.5, water-to-material ratio of 3:4, grinding ball particle size and grading of 18-22 mm:9-11 mm:3.5-4 mm = 3:6:1, and the ball mill speed of 400 r / min.
[0037] (2) Take 27 parts of the micropowder slurry obtained in step (1), mix with 63 parts of cement and 16 parts of water, and obtain a cement-recycled micropowder sample after vibration, molding and curing. The curing conditions are: the temperature is 20±2°C and the humidity is not less than 95% within 28 days. Comparative Example 1: No wet grinding, dry grinding and triethanolamine reaction conditions
[0038] Take 20 parts of recycled micro powder with a particle size less than 0.16 mm, mix with 63 parts of cement and 36 parts of water, and obtain cement-recycled micro powder samples after vibration, molding and curing. The curing conditions are: the temperature is 20±2℃ and the humidity is not less than 95% within 28 days. Comparative Example 2: No wet grinding and triethanolamine reaction conditions
[0039] (1) Take 20 portions of regenerated micro powder with a particle size less than 0.16 mm and dry grind for 30 minutes to obtain regenerated micro powder with a finer median particle size. The dry grinding conditions are: ball-to-material ratio is 1:2.5, grinding ball particle size and gradation are 18-22mm:9-11mm:3.5-4mm = 3:6:1, and the ball mill speed is 400r / min.
[0040] (2) Take 27 parts of the fine powder obtained in step (1), mix with 63 parts of cement and 36 parts of water, and obtain a cement-regenerated fine powder sample after vibration, molding and curing. The curing conditions are: the temperature is 20±2°C and the humidity is not less than 95% within 28 days.
[0041] Table 1 below shows the components and their mass fractions in the above examples and comparative examples. Table 2 shows the test results of the pure pulp properties prepared by the physical-chemical method for improving the activity of the regenerated micropowder obtained in the above examples and comparative examples.
[0042]
[0043]
[0044] It can be seen from Table 1 that by using wet grinding and triethanolamine, the ion dissolution of the regenerated micropowder continues to increase, the solubility of active calcium ions, silicon ions and aluminum ions continues to increase, and the activity of the micropowder also continues to increase accordingly.
[0045] As can be seen from Table 2, the activity index of the auxiliary cementitious materials prepared in Examples 1-4 of the present invention is greater than 70%, which is better than 65% in the comparative example, and meets the standards of common auxiliary cementitious materials such as fly ash and steel slag. In addition, the method avoids the high energy consumption of high-temperature preparation during the preparation process and adopts a simple wet grinding colloid preparation process, which reduces the production cost and has significant social and environmental benefits.
[0046] Depend on Figure 1 It can be seen that the slurry prepared by the present invention can indirectly adjust the setting time by adjusting the dosage of the admixture, indicating that increasing the dosage of the admixture can reduce the final setting time of the slurry out of Ninghe River, thereby meeting the use of cementitious materials in different environments.
[0047] Although the present invention is disclosed as above with preferred embodiments, it is not intended to limit the scope of the present invention. Any person skilled in the art can make some improvements without departing from the scope of the present invention, that is, all equivalent improvements made according to the present invention should be covered by the scope of the present invention.
Claims
1. A method for physical-chemical combined activation and regeneration of regenerated micropowder, Features The steps include: Step 1: Collect the demolished construction waste and place it in a multi-stage crusher to obtain waste concrete recycled micro powder through crushing, screening and sorting; Step 2: Take 10-25 parts of waste concrete recycled micro powder and mix it with 10-45 parts of water, add 0.02-0.2 parts of chemical admixture, and wet-ball mill for 30 minutes to obtain recycled micro powder slurry; Step 3: Mix 10-30 parts of the regenerated micropowder slurry with 60-90 parts of cement and 5-40 parts of water, and then pour the obtained cement-micropowder slurry into a mold for molding, and obtain the cement-micropowder pure slurry material through vibration and curing.
2. The method according to claim 1, Features: In step 1, the particle size of the waste concrete recycled fine powder is ≤0.16 mm.
3. The method according to claim 1, Features: In step 2, the chemical admixture is one or more alcoholamine or phosphoric acid group substances having hydroxyl, amine and phosphoric acid groups, which have grinding aid and chemical complexing effects.
4. The method according to claim 3, Features: The chemical additive is selected from one or more of triethanolamine and triisopropanolamine.
5. The method according to claim 1, Features: In step 2, during wet ball milling, the ball-to-material ratio in the ball mill is 1:1-3:
1.
6. The method according to claim 5, Features: The grinding balls are made of zirconium oxide with a gradation of 18-22mm:9-11mm:3.5-4mm = 3:6:1, and the ball mill speed is 400r / min.
7. The method according to claim 1, Features: In step 3, the test block needs to be cured for 24 hours before demolding and for 28 days after demolding. The curing environment is 20±2℃ and the humidity is not less than 95%.
Citation Information
Patent Citations
Method for preparing building mortar through building rubbish
CN106242336A
Construction waste micro-powder carbonization and reactivation method
CN116283022A