Anti-crack gypsum-based self-leveling mortar and preparation method thereof
By using activated polyacrylonitrile fibers, steel slag sand and steel slag powder in gypsum-based self-leveling mortar, a metal chelate fiber network is formed, which solves the problems of insufficient crack resistance and fluidity in the prior art, and achieves high pressure resistance Mortar with strength, flexural strength and fluidity reduces production costs.
Patent Information
- Application Number
- CN202411159707.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
AI Technical Summary
The existing gypsum-based self-leveling mortar has difficulties in improving crack resistance and fluidity, and due to the high additive cost and high application cost, it limits its promotion.
Activated polyacrylonitrile fibers, steel slag sand and steel slag powder are used as the main raw materials. Through specific mixing and treatment methods, a stable metal chelate fiber network is formed to enhance the mechanical properties of the mortar and reduce production costs.
The compressive strength, flexural strength and fluidity of the self-leveling mortar of crack-resistant gypsum are significantly improved, the production cost is reduced, the water retention capacity is improved, the problem of uneven fiber dispersion is avoided, and the overall performance of the mortar is improved.
Smart Images

Figure BDA0005006088580000071 
Figure BDA0005006088580000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to a crack-resistant gypsum-based self-leveling mortar and a preparation method thereof. Background Art
[0002] Self-leveling mortar is a new type of functional building mortar recognized as a high value-added material and has been widely used in recent years. Self-leveling mortar has good fluidity and self-leveling properties. It is self-leveling in the fresh state, has high early strength, smooth surface, and stable volume change in the hardened state. It has unique performance and advantages of saving cost and manpower in engineering applications.
[0003] Gypsum-based self-leveling mortar is made of high-strength gypsum, cement, fine aggregate and various building chemical additives. Gypsum-based self-leveling has the advantages of high levelness and not easy to hollow and crack. Most manufacturers use building gypsum to prepare and rely on increasing the amount of chemical additives to ensure that the corresponding performance requirements are met. The cost of additives accounts for about two-thirds of the production cost of self-leveling gypsum, resulting in the application cost of self-leveling gypsum being higher than cement mortar, and the promotion and application are hindered and the development is slow.
[0004] Adding polyacrylonitrile fiber to mortar can significantly improve toughness, refine cracks, reduce the risk of cracking of cement-based materials, and even make the mortar present strain hardening mechanical characteristics, that is, when the material is uniaxially stretched, before the ultimate tensile strain is reached, the stress increases with the strain. Its formation mechanism is that many fine cracks are formed during the tension of the material without reducing the bearing capacity. However, the bonding and water retention of polyacrylonitrile fiber and mortar are poor, which has a great influence on the fluidity of the mortar.
[0005] Therefore, the applicant prepared a crack-resistant gypsum-based self-leveling mortar to solve the above problems. Summary of the invention
[0006] In order to solve the existing technical problems, the present invention provides a crack-resistant gypsum-based self-leveling mortar. The raw material components include, by weight: 100 parts by weight of mixed cement, 200-350 parts by weight of α-high-strength gypsum, 260-300 parts by weight of steel slag sand, 140 parts by weight of steel slag powder, 1-3 parts by weight of water reducer, 10-25 parts by weight of activated polyacrylonitrile fiber, 190 parts by weight of water, and 0.5-1 parts by weight of defoamer; the crack resistance and fluidity of the crack-resistant gypsum-based self-leveling mortar are enhanced by adding activated polyacrylonitrile fiber.
[0007] Furthermore, the mixed cement is obtained by mixing silicate cement and aluminate cement in a mass ratio of 1:0.08-0.1.
[0008] Furthermore, the particle size of the steel slag sand is 0.15-0.60 mm; the wear resistance of the steel slag sand is better than that of conventional quartz sand.
[0009] Furthermore, the particle size of the steel slag powder is 0.09-0.2 mm.
[0010] The steel slag sand is obtained by crushing steel slag; the steel slag powder is obtained by crushing and grinding steel slag; the steel slag is collected from the steel slag produced by Jiangsu Yancheng Lianxin Iron and Steel Co., Ltd., with an aging time of 3 years and magnetic separation; the raw material steel slag of the steel slag sand and steel slag powder of the present invention has a long aging time, so the relative activity is low and the volume stability is also good, so the steel slag can be used as aggregate for self-leveling mortar.
[0011] Furthermore, the activated polyacrylonitrile fiber is obtained by activating the polyacrylonitrile fiber in a hydroxylamine hydrochloride solution.
[0012] The present invention also provides a method for preparing a crack-resistant gypsum-based self-leveling mortar, comprising the following preparation steps:
[0013] (1) Ingredients: weigh and prepare the ingredients according to the weight proportions of the raw material components described in claim 1;
[0014] (2) primary mixing: 10-25 parts by weight of activated polyacrylonitrile fiber and 90 parts by weight of deionized water are stirred and mixed at 1200-1600 r / min for 20-40 min, then 25% hydrochloric acid is added to adjust the pH to 5-6, stirring is continued for 10-30 min, the temperature is raised to 60° C., 140 parts of steel slag powder is added, stirring is continued at 600-800 r / min for 1-3 h, then 260-300 parts of steel slag sand is added, stirring is continued at 400-600 r / min for 20-40 min, and the mixture is naturally cooled to room temperature to obtain a primary mixture;
[0015] (3) 100 parts by mass of mixed cement and 200-350 parts by mass of α-high-strength gypsum are stirred and mixed uniformly at 100-200 r / min for 1-3 min, followed by adding 100 parts by mass of water, 1-3 parts by mass of water reducing agent, and 0.5-1 parts by mass of defoaming agent in sequence, and the stirring and mixing is continued for 1-3 min. Then, the mixture is added once while stirring at 400-600 r / min and then stirred for 1-1.5 min. The mortar is stirred into a uniform fluid state, poured evenly on the construction surface, and allowed to level naturally. A defoaming roller is used to roll on it to release air, and it is naturally cured after leveling to obtain a crack-resistant gypsum-based self-leveling mortar.
[0016] Furthermore, the preparation method of the activated polyacrylonitrile fiber is as follows: add the polyacrylonitrile fiber to a 30g / L hydroxylamine hydrochloride solution of 40 to 60 times its mass, adjust the pH to 6 with 25% hydrochloric acid and 25% ammonia water, then place it in a 70°C oscillating water bath to react for 2 hours, filter it out and soak it in deionized water for 30 minutes, then rinse it with deionized water several times until the rinsed liquid is neutral, and then dry it in a blast drying oven for 12 hours to obtain activated polyacrylonitrile fiber.
[0017] Furthermore, the polyacrylonitrile fiber has a length of 6 mm, a fineness of 1.9, and a specific gravity of 1.18 g / cm 3 , the tensile strength is 330~413MPa, the elastic modulus is 12100~17100MPa, and the elongation is 14~20%.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The invention first mixes activated polyacrylonitrile fiber, water, steel slag sand and steel slag powder, and then mixes other raw materials and adds them into the mixed material to prepare the anti-cracking gypsum-based self-leveling mortar, which has good fluidity, wear resistance and crack resistance, and high compressive strength and flexural strength.
[0020] The anti-cracking gypsum-based self-leveling mortar prepared by the present invention adds steel slag sand and steel slag powder instead of quartz sand and heavy calcium powder, so that the wear resistance of the anti-cracking gypsum-based self-leveling mortar can be improved. Although the activity of the steel slag powder is relatively low, it still has a certain hydration activity compared with the heavy calcium powder used as a filler, and has the function of enhancing the later strength of the cement-based self-leveling mortar. Since the surface of the steel slag sand contains active clinker mineral components, their hydration enhances the bonding between the steel slag sand particles and the cement paste. Due to the roughness and irregularity of the surface morphology of the steel slag sand, the bite force between the particles and the ability to combine with the cement-based cementitious material are higher than those of the natural quartz sand with a smooth surface. The mortar also has multiple functions such as reducing production costs, saving natural quartz sand and limestone resources, and protecting the environment.
[0021] Activated polyacrylonitrile fibers are added to the crack-resistant gypsum-based self-leveling mortar prepared by the present invention, and a large number of amino and amidoxime groups are generated on the surface of polyacrylonitrile. During subsequent mixing, the amino and amidoxime groups are combined with free iron ions in steel slag sand and steel slag powder by coordination bonds to form a stable metal chelate fiber network, which is cross-linked with the network gel of the mortar, thereby enhancing the mechanical properties of the mortar. At this time, metal ions are chelated on the side chains of the fibers, and the empty orbitals on the periphery thereof can be complexed with water molecules, and the polar structure thereof can also produce a dipole effect with polar water molecules, making the fibers easier to react with water, thereby forming a layer of water film that can fix a large amount of water, thereby making the entire gypsum-based self-leveling mortar have good water retention capacity, thereby improving the fluidity of the gypsum-based self-leveling mortar, and uniformly dispersing the polyacrylonitrile fibers in the mortar, thereby avoiding the problem that the fluidity of the mortar, the crack resistance, the compressive strength and the flexural strength are affected due to the entanglement and uneven dispersion of the polyacrylonitrile fibers. DETAILED DESCRIPTION
[0022] The present invention is further described in detail below in conjunction with examples, but the following examples should not be construed as limiting the present invention.
[0023] Some of the raw materials of the embodiments of the present invention and the comparative examples are as follows:
[0024] The silicate cement is P.O42.5 grade ordinary silicate cement produced by Kaifeng Jingyu Mengdian Cement Co., Ltd., and its specific surface area is 380m 2 / kg;
[0025] The aluminate cement is a CA50-J9 aluminate cement produced by Henan Dengfeng Melting Material Co., Ltd., produced by sintering method, with a specific surface area of not less than 400m 2 / kg.
[0026] The standard consistency of the α-high-strength gypsum is 30% to 40%, the initial setting time is 6 to 8 minutes, the final setting time is 20 to 30 minutes, and the 2h flexural strength is 8MPa;
[0027] The natural quartz sand is commercially available river sand, and particles with a particle size of 0.16 to 0.63 mm are sieved;
[0028] The density of the heavy calcium powder is 2.65 g / cm 3 , with a specific surface area of 355m 2 / kg;
[0029] The steel slag sand is obtained by crushing the steel slag with a jaw crusher and then sieving out particles with a particle size of 0.15 to 0.60 mm.
[0030] The steel slag powder is crushed and ground to obtain steel slag powder with a particle size of 0.09 to 0.2 mm;
[0031] The steel slag is collected from the steel slag produced by Jiangsu Yancheng Lianxin Steel Co., Ltd., aged for 3 years, and subjected to magnetic separation.
[0032] The water reducing agent adopts the polycarboxylic acid high-performance water reducing agent of BASF of Germany, with a water reduction rate of 28%, a water bleeding rate of 45%, an air content of 5.0%, a setting time difference of 100 minutes for initial setting and 90 minutes for final setting.
[0033] The water retaining agent is P4123 from Hercules, hydroxypropyl methylcellulose, and a 2% aqueous solution with a viscosity of 40,000 cps (Brookfield RVT, 20° C., test average).
[0034] The defoamer is BASF's defoamer FoamStar ST2438.
[0035] The polyacrylonitrile fiber has a length of 6 mm, a fineness of 1.9, and a specific gravity of 1.18 g / cm 3 , the tensile strength is 330~413MPa, the elastic modulus is 12100~17100MPa, and the elongation is 14~20%.
[0036] The water used shall be tap water that complies with the provisions of JGJ63-2006 "Standard for Water Used in Concrete Mixing";
[0037] Example 1
[0038] A method for preparing anti-cracking gypsum-based self-leveling mortar, the preparation steps are as follows:
[0039] (1) Ingredients: The ingredients are weighed and prepared according to the weight proportions of the following raw material components: 100 parts by weight of mixed cement, 200 parts by weight of α-high-strength gypsum, 260 parts by weight of steel slag sand, 140 parts by weight of steel slag powder, 1 part by weight of water reducer, 10 parts by weight of activated polyacrylonitrile fiber, 190 parts by weight of water, and 0.5 parts by weight of defoamer;
[0040] (2) Primary mixing: 10 parts by weight of activated polyacrylonitrile fiber and 90 parts by weight of deionized water were stirred and mixed at 1200 r / min for 20 min, followed by adding 25% hydrochloric acid to adjust the pH to 5, and stirring was continued for 10 min. The mixture was heated to 60° C., 140 parts by weight of steel slag powder was added, and stirring was continued at 600 r / min for 1 h. Subsequently, 260 parts by weight of steel slag sand was added, and stirring was continued at 400 r / min for 20 min. The mixture was naturally cooled to room temperature to obtain a primary mixture.
[0041] (3) 100 parts by weight of mixed cement and 200 parts by weight of α-high-strength gypsum were stirred and mixed uniformly at 100 r / min for 1 min, followed by adding 100 parts by weight of water, 1 part by weight of water reducer, and 0.5 parts by weight of defoamer in sequence, and continued to stir and mix for 1 min, then adding the primary mixture while stirring at 400 r / min and stirring for another 1 min, stirring the mortar into a uniform fluid state, pouring it evenly on the construction surface, allowing it to level naturally, rolling it with a defoaming roller to deflate it, and naturally curing it after leveling to obtain a crack-resistant gypsum-based self-leveling mortar;
[0042] The mixed cement is obtained by mixing silicate cement and aluminate cement in a mass ratio of 1:0.08;
[0043] The preparation method of the activated polyacrylonitrile fiber is as follows: adding the polyacrylonitrile fiber to a 30g / L hydroxylamine hydrochloride solution of 40 times its mass, adjusting the pH to 6 with 25% hydrochloric acid and 25% ammonia water, then placing it in a 70°C shaking water bath for reaction for 2h, filtering it out and then soaking it in deionized water for 30min, then rinsing it with deionized water for multiple times until the rinsed liquid is neutral, and then drying it in a forced air drying oven for 12h to obtain the activated polyacrylonitrile fiber.
[0044] Example 2
[0045] A method for preparing anti-cracking gypsum-based self-leveling mortar, the preparation steps are as follows:
[0046] (1) Ingredients: The ingredients are weighed and prepared according to the weight proportions of the following raw material components: 100 parts by weight of mixed cement, 280 parts by weight of α-high-strength gypsum, 280 parts by weight of steel slag sand, 140 parts by weight of steel slag powder, 2 parts by weight of water reducer, 15 parts by weight of activated polyacrylonitrile fiber, 190 parts by weight of water, and 0.7 parts by weight of defoamer;
[0047] (2) Primary mixing: 15 parts by mass of activated polyacrylonitrile fiber and 90 parts by mass of deionized water were stirred and mixed at 1400 r / min for 30 min, followed by adding 25% hydrochloric acid to adjust the pH to 6, and stirring was continued for 20 min. The mixture was heated to 60° C., 140 parts by mass of steel slag powder was added, and stirring was continued at 700 r / min for 2 h. Subsequently, 280 parts by mass of steel slag sand was added, and stirring was continued at 500 r / min for 30 min. The mixture was naturally cooled to room temperature to obtain a primary mixture.
[0048] (3) 100 parts by weight of mixed cement and 280 parts by weight of α-high-strength gypsum were stirred and mixed uniformly at 150 r / min for 2 min, followed by adding 100 parts by weight of water, 2 parts by weight of water reducer, and 0.7 parts by weight of defoamer in sequence, and continued to stir and mix for 2 min, then adding the primary mixture while stirring at 500 r / min, and then stirring for another 1.3 min, stirring the mortar into a uniform fluid state, pouring it evenly on the construction surface, allowing it to level naturally, rolling it with a defoaming roller to deflate it, and naturally curing it after leveling to obtain a crack-resistant gypsum-based self-leveling mortar;
[0049] The mixed cement is obtained by mixing silicate cement and aluminate cement in a mass ratio of 1:0.09;
[0050] The preparation method of the activated polyacrylonitrile fiber is as follows: adding the polyacrylonitrile fiber to a 30g / L hydroxylamine hydrochloride solution of 50 times its mass, adjusting the pH to 6 with 25% hydrochloric acid and 25% ammonia water, then placing it in a 70°C shaking water bath for reaction for 2h, filtering it out and then soaking it in deionized water for 30min, then rinsing it with deionized water for multiple times until the rinsed liquid is neutral, and then drying it in a forced air drying oven for 12h to obtain the activated polyacrylonitrile fiber.
[0051] Example 3
[0052] (1) Ingredients: Weigh and prepare the ingredients according to the weight proportions of the following raw material components: 100 parts by weight of mixed cement, 350 parts by weight of α-high-strength gypsum, 300 parts by weight of steel slag sand, 140 parts by weight of steel slag powder, 3 parts by weight of water reducer, 25 parts by weight of activated polyacrylonitrile fiber, 190 parts by weight of water, and 1 part by weight of defoamer;
[0053] (2) Primary mixing: 25 parts by mass of activated polyacrylonitrile fiber and 90 parts by mass of deionized water were stirred and mixed at 1600 r / min for 40 min, followed by adding 25% hydrochloric acid to adjust the pH to 6, and stirring was continued for 30 min. The mixture was heated to 60° C., 140 parts by mass of steel slag powder was added, and stirring was continued at 800 r / min for 3 h. Subsequently, 300 parts by mass of steel slag sand was added, and stirring was continued at 600 r / min for 40 min. The mixture was naturally cooled to room temperature to obtain a primary mixture.
[0054] (3) 100 parts by weight of mixed cement and 350 parts by weight of α-high-strength gypsum were stirred and mixed uniformly at 200 r / min for 3 min, followed by adding 100 parts by weight of water, 3 parts by weight of water reducer, and 1 part by weight of defoamer in sequence, and continued to stir and mix for 3 min, then adding the primary mixture while stirring at 600 r / min and stirring for another 1.5 min, stirring the mortar into a uniform fluid state, pouring it evenly on the construction surface, allowing it to level naturally, rolling it with a defoaming roller to deflate it, and naturally curing it after leveling to obtain a crack-resistant gypsum-based self-leveling mortar;
[0055] The mixed cement is obtained by mixing silicate cement and aluminate cement in a mass ratio of 1:0.1;
[0056] The preparation method of the activated polyacrylonitrile fiber is as follows: adding the polyacrylonitrile fiber to a 30g / L hydroxylamine hydrochloride solution of 60 times its mass, adjusting the pH to 6 with 25% hydrochloric acid and 25% ammonia water, then placing it in a 70°C shaking water bath for reaction for 2 hours, filtering it out and then soaking it in deionized water for 30 minutes, then rinsing it with deionized water for multiple times until the rinsed liquid is neutral, and then drying it in a forced air drying oven for 12 hours to obtain the activated polyacrylonitrile fiber.
[0057] Comparative Example 1
[0058] The only difference between Comparative Example 1 and Example 2 is that the raw material components include: 100 parts by mass of mixed cement, 280 parts by mass of α-high-strength gypsum, 280 parts by mass of natural quartz sand, 140 parts by mass of heavy calcium powder, 2 parts by mass of water reducer, 15 parts by mass of activated polyacrylonitrile fiber, 190 parts by mass of water, and 0.7 parts by mass of defoaming agent, and the remaining steps and ingredients are the same as those in Example 2.
[0059] Comparative Example 2
[0060] The only difference between Comparative Example 2 and Example 2 is that polyacrylonitrile is used to prepare the anti-cracking gypsum-based self-leveling mortar, and the remaining steps and ingredients are the same as those in Example 2.
[0061] Comparative Example 3
[0062] (1) Ingredients: The ingredients are weighed and prepared according to the weight proportions of the following raw material components: 100 parts by weight of mixed cement, 280 parts by weight of α-high-strength gypsum, 280 parts by weight of steel slag sand, 140 parts by weight of steel slag powder, 2 parts by weight of water reducer, 15 parts by weight of activated polyacrylonitrile fiber, 190 parts by weight of water, and 0.7 parts by weight of defoamer;
[0063] (3) 100 parts by weight of mixed cement, 280 parts by weight of α-high-strength gypsum, 15 parts by weight of activated polyacrylonitrile fiber, 140 parts by weight of steel slag powder, and 280 parts by weight of steel slag sand were stirred and mixed uniformly at 150 r / min for 2 min, and then 190 parts by weight of water, 2 parts by weight of water reducer, and 0.7 parts by weight of defoamer were added in sequence, and the stirring and mixing continued for 2 min, and then the mixture was added once while stirring at 500 r / min and then stirred for 1.3 min, and the mortar was stirred into a uniform fluid state, and evenly poured on the construction surface to make it naturally leveled, and a defoaming roller was used to roll on it to deflate, and naturally cured after leveling to obtain a crack-resistant gypsum-based self-leveling mortar;
[0064] The mixed cement is obtained by mixing silicate cement and aluminate cement in a mass ratio of 1:0.09;
[0065] The preparation method of the activated polyacrylonitrile fiber is as follows: adding the polyacrylonitrile fiber to a 30g / L hydroxylamine hydrochloride solution of 50 times its mass, adjusting the pH to 6 with 25% hydrochloric acid and 25% ammonia water, then placing it in a 70°C shaking water bath for reaction for 2h, filtering it out and then soaking it in deionized water for 30min, then rinsing it with deionized water for multiple times until the rinsed liquid is neutral, and then drying it in a forced air drying oven for 12h to obtain the activated polyacrylonitrile fiber.
[0066] Comparative Example 4
[0067] The difference between Comparative Example 4 and Example 2 is that the raw material components, by weight, include: 100 parts by weight of mixed cement, 280 parts by weight of α-high-strength gypsum, 280 parts by weight of steel slag sand, 140 parts by weight of steel slag powder, 2 parts by weight of water reducer, 0.8 parts by weight of water retaining agent, 15 parts by weight of polyacrylonitrile fiber, 190 parts by weight of water, and 0.7 parts by weight of defoaming agent. The remaining steps and ingredients are the same as those in Example 2.
[0068] Effect example
[0069] Table 1 below shows the performance test analysis results of the anti-cracking gypsum-based self-leveling mortars prepared by Examples 1 to 3 and Comparative Examples 1 to 4 of the present invention.
[0070] Table 1
[0071]
[0072]
[0073] From Table 1, it can be found that the anti-cracking gypsum-based self-leveling mortar prepared in the embodiment has high compressive strength and flexural strength, good fluidity, crack resistance and wear resistance; Example 2 is compared with Comparative Example 1 to find that the anti-cracking gypsum-based self-leveling mortar prepared with steel slag sand and steel slag powder has high compressive strength and flexural strength, good fluidity, crack resistance and wear resistance; Example 2 is compared with Comparative Examples 2 and 4 to find that the anti-cracking gypsum-based self-leveling mortar prepared with activated polyacrylonitrile fiber has good fluidity and crack resistance; Example 2 is compared with Comparative Example 3 to find that the anti-cracking gypsum-based self-leveling mortar prepared by one-time mixing has high compressive strength and flexural strength, good fluidity and crack resistance.
[0074] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
Claims
1. A crack-resistant gypsum-based self-leveling mortar, characterized in that: In terms of weight, the raw material components include: 100 parts by weight of mixed cement, 200-350 parts by weight of α-high-strength gypsum, 260-300 parts by weight of steel slag sand, 140 parts by weight of steel slag powder, 1-3 parts by weight of water reducer, 10-25 parts by weight of activated polyacrylonitrile fiber, 190 parts by weight of water, and 0.5-1 parts by weight of defoaming agent.
2. The anti-cracking gypsum-based self-leveling mortar according to claim 1, characterized in that: The mixed cement is obtained by mixing silicate cement and aluminate cement in a mass ratio of 1:0.08-0.
1.
3. The anti-cracking gypsum-based self-leveling mortar according to claim 1, characterized in that: The particle size of the steel slag sand is 0.15-0.60 mm.
4. The anti-cracking gypsum-based self-leveling mortar according to claim 1, characterized in that: The particle size of the steel slag powder is 0.09-0.2 mm.
5. The anti-cracking gypsum-based self-leveling mortar according to claim 1, characterized in that: The activated polyacrylonitrile fiber is obtained by activating the polyacrylonitrile fiber in a hydroxylamine hydrochloride solution.
6. A method for preparing the anti-cracking gypsum-based self-leveling mortar according to any one of claims 1 to 5, characterized in that: The method comprises the following preparation steps: (1) Ingredients: weigh and prepare the ingredients according to the weight proportions of the raw material components described in claim 1; (2) primary mixing: 10-25 parts by weight of activated polyacrylonitrile fiber and 90 parts by weight of deionized water are stirred and mixed at 1200-1600 r / min for 20-40 min, then 25% hydrochloric acid is added to adjust the pH to 5-6, stirring is continued for 10-30 min, the temperature is raised to 60° C., 140 parts of steel slag powder is added, stirring is continued at 600-800 r / min for 1-3 h, then 260-300 parts of steel slag sand is added, stirring is continued at 400-600 r / min for 20-40 min, and the mixture is naturally cooled to room temperature to obtain a primary mixture; (3) 100 parts by mass of mixed cement and 200-350 parts by mass of α-high-strength gypsum are stirred and mixed uniformly at 100-200 r / min for 1-3 min, followed by adding 100 parts by mass of water, 1-3 parts by mass of water reducing agent, and 0.5-1 parts by mass of defoaming agent in sequence, and the stirring and mixing is continued for 1-3 min. Then, the mixture is added once while stirring at 400-600 r / min and then stirred for 1-1.5 min. The mortar is stirred into a uniform fluid state, poured evenly on the construction surface, and allowed to level naturally. A defoaming roller is used to roll on it to release air, and it is naturally cured after leveling to obtain a crack-resistant gypsum-based self-leveling mortar.
7. The method for preparing the anti-cracking gypsum-based self-leveling mortar according to claim 6, characterized in that: The preparation method of the activated polyacrylonitrile fiber is as follows: adding the polyacrylonitrile fiber to a 30g / L hydroxylamine hydrochloride solution of 40 to 60 times its mass, adjusting the pH to 6 with 25% hydrochloric acid and 25% ammonia water, then placing it in a 70°C shaking water bath for reaction for 2 hours, filtering it out and then soaking it in deionized water for 30 minutes, then rinsing it with deionized water for multiple times until the rinsed liquid is neutral, and then drying it in a forced air drying oven for 12 hours to obtain the activated polyacrylonitrile fiber.
8. The method for preparing the anti-cracking gypsum-based self-leveling mortar according to claim 7, characterized in that: The polyacrylonitrile fiber has a length of 6 mm, a fineness of 1.9, and a specific gravity of 1.18 g / cm 3 , the tensile strength is 330~413MPa, the elastic modulus is 12100~17100MPa, and the elongation is 14~20%.
Citation Information
Cited By
Steel slag wear-resistant sand as well as preparation method and construction method thereof