Aluminum-doped zinc oxide nano-powder as well as preparation method and application thereof

Through the preparation of aluminum-doped zinc oxide nano powder, the problem that zinc oxide targets cannot meet the thickness and flatness of high-frequency coatings is solved, and the signal reception capacity of high-efficiency thin-film bulk acoustic wave resonators is achieved, reducing costs and ensuring Stability of coating.

CN118908718APending Publication Date: 2024-11-08PEAK RUI RONGZE (HANGZHOU) ENTERPRISE CONSULTING MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410983818.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In existing high-frequency thin film bulk acoustic resonators, zinc oxide targets cannot meet the needs of coating thickness and surface flatness, resulting in insufficient signal reception capacity and high cost, making it difficult to achieve mass production.

Method used

Aluminum-doped zinc oxide nanopowder is used to mix zinc oxide and alumina, and add dispersant, binder and defoaming agent, and then prepare by grinding and centrifugal spray-drying to form a compactness of 1.2-1.4g/cm3. Solid sphere nanopowder is used to prepare piezoelectric film magnetron sputtering targets to achieve stability of thick coatings above 400nm.

Benefits of technology

The prepared ceramic target has a more uniform crystalline microstructure and small crystal size, which can achieve a stable thick coating on large-sized silicon wafers, avoid cracking and film delamination, and improve signal reception capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908718A_ABST
    Figure CN118908718A_ABST
Patent Text Reader

Abstract

The invention discloses aluminum-doped zinc oxide nano-powder and a preparation method and application thereof, the nano-powder is solid powder, the D50 of the nano-powder is 10-30 [mu] m, and the compactness of the nano-powder is 1.2-1.4 g / cm < 3 >. The invention has the beneficial effects that the nano-powder is a solid sphere, the D50 of the nano-powder is 10-30 [mu] m, and the compactness of the nano-powder is 1.2-1.4 g / cm < 3 >. The nano powder body can be sintered to produce a ceramic target material with a more uniform crystal microstructure and a smaller crystal size, and the obtained ceramic target material can realize a stable thick coating film of more than 400 nanometers on a large-size silicon wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to aluminum-doped zinc oxide nano powder and a preparation method and application thereof. Background Art

[0002] A film bulk acoustic wave resonator is a resonator based on sound waves, usually composed of a film and a substrate. Its working principle is based on the propagation of elastic waves in a film. When an electric field is applied or the film is excited by the piezoelectric effect, sound waves will be generated in the film, and these sound waves will be reflected between the film and the substrate and form resonance.

[0003] At present, the mainstream high-frequency (5G) thin-film bulk acoustic wave resonators on the market mainly use aluminum scandium nitride materials. The technology is mature, but there is no relevant report on the intellectual property rights of the material coating technology in my country. Aluminum scandium nitride is expensive due to the use of a large amount of scandium metal. Although many academic papers have demonstrated the 5G frequency band reception capability of zinc oxide piezoelectric films, mass production has not been achieved because large-sized magnetron sputtering targets are required to produce large-sized coated wafers for processing resonators, and the quality requirements for the targets are extremely high. The zinc oxide targets available on the market cannot meet the needs of high-frequency wireless communication coating, such as insufficient coating thickness (above 400nm can reach 800nm ​​as preferred) and the formation of large-area and uniformly thick coatings. In addition, the surface flatness of the sputtered films of zinc oxide targets available on the market is not good, and signals cannot be effectively received. Films with a thickness of more than 400nm are very easy to crack and peel off and become scrapped. Summary of the invention

[0004] The invention provides an aluminum-doped zinc oxide nano powder and a preparation method and application thereof.

[0005] In a first aspect of the present invention, there is provided an aluminum-doped zinc oxide nanopowder, wherein the nanopowder is a solid powder, the D50 of the nanopowder is 10-30 um, and the density of the nanopowder is 1.2-1.4 g / cm 3 , for example 1.2 g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 .

[0006] According to some embodiments of the nanopowder of the present invention, raw materials for preparing the nanopowder include zinc oxide and aluminum oxide.

[0007] According to some embodiments of the nanopowder of the present invention, the raw materials for preparing the nanopowder further include a dispersant, a binder and a defoaming agent.

[0008] According to some embodiments of the nanopowder of the present invention, the dispersant is selected from water and / or SD-3 organic bentonite dispersant.

[0009] According to some embodiments of the nanopowder of the present invention, the water is deionized water.

[0010] According to some embodiments of the nanopowder of the present invention, the binder is PVA glue.

[0011] According to some embodiments of the nanopowder of the present invention, the defoaming agent is n-butanol.

[0012] According to some embodiments of the nanopowder of the present invention, the weight ratio of zinc oxide to aluminum oxide in the raw materials for preparing the nanopowder is (95-99.5):(5-0.5), preferably 98:2.

[0013] According to some embodiments of the nanopowder of the present invention, the weight ratio of the dispersant, the binder, the defoaming agent and the aluminum oxide in the raw materials for preparing the nanopowder is: (0.3-1.1): (2-9): (0.02-0.04): 1.

[0014] According to some embodiments of the nanopowder of the present invention, the weight ratio of the dispersant, the binder, the defoaming agent and the aluminum oxide in the raw materials for preparing the nanopowder is 0.38:9:0.02:1.

[0015] According to some embodiments of the nanopowder of the present invention, the weight ratio of the dispersant, the binder, the defoaming agent and the aluminum oxide in the raw materials for preparing the nanopowder is 0.38:4.5:0.02:1.

[0016] The second aspect of the present invention provides a method for preparing the nanopowder according to the first aspect of the present invention, comprising the following steps:

[0017] (1) mixing zinc oxide, aluminum oxide, a dispersant and a defoaming agent and grinding them to obtain a mixture;

[0018] (2) mixing the mixture obtained in step (1) with a binder to obtain a slurry;

[0019] (3) Drying and granulating the slurry obtained in step (2) to obtain the aluminum-doped zinc oxide nanopowder.

[0020] According to some embodiments of the preparation method of the present invention, in step (1), the particle size of the zinc oxide is 0.8-1.2 um, and the particle size of the aluminum oxide is 0.8-1.2 um.

[0021] According to some embodiments of the preparation method of the present invention, the grinding medium used in the grinding is zirconium oxide.

[0022] According to some embodiments of the preparation method of the present invention, the particle size of the zirconium oxide is 2-3 mm, for example, 2 mm, 2.5 mm, 3 mm; preferably 3 mm.

[0023] According to some embodiments of the preparation method of the present invention, the grinding rotation speed is 30-50 r / min, for example, 30 r / min, 35 r / min, 40 r / min, 45 r / min, 50 r / min.

[0024] According to some embodiments of the preparation method of the present invention, the grinding time is 20-28 hours, for example, 20 hours, 25 hours, 26 hours, 28 hours.

[0025] According to some embodiments of the preparation method of the present invention, the pH of the slurry is 8-9.5.

[0026] According to some embodiments of the preparation method of the present invention, in step (3), the drying is centrifugal spray drying.

[0027] According to some embodiments of the preparation method of the present invention, the inlet air temperature of the centrifugal spray drying is 150-300°C, for example, 200°C, 220°C, 250°C, 260°C, 280°C, 300°C, preferably 260°C.

[0028] According to some embodiments of the preparation method of the present invention, the atomization frequency of the centrifugal spray drying is 250-350 Hz, 250 Hz, 280 Hz, 300 Hz, 320 Hz, or 350 Hz.

[0029] The third aspect of the present invention provides an application of the aluminum-doped zinc oxide nanopowder described in the first aspect of the present invention or the aluminum-doped zinc oxide nanopowder obtained by the preparation method described in the second aspect of the present invention in piezoelectric film magnetron sputtering targets.

[0030] According to some embodiments of the application of the present invention, the size of the piezoelectric film magnetron sputtering target is 250-260 mm.

[0031] The beneficial effects of the present invention are as follows: the nano powder of the present invention is a solid sphere, its D50 is 10-30um, and its density is 1.2-1.4g / cm 3 The nano powder can produce a ceramic target material with a more uniform crystal microstructure and a smaller crystal size through sintering, and the obtained ceramic target material can achieve a stable coating thickness of more than 400 nanometers on a large-size silicon wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the distribution diagram of the powder D50 prepared in Example 1 of the present application;

[0033] Figure 2 This is a SEM image of the powder prepared in Example 1 of the present application magnified 100 times;

[0034] Figure 3 This is a SEM image of the powder prepared in Example 1 of the present application magnified 1000 times;

[0035] Figure 4 This is a SEM image of the powder prepared in Comparative Example 1 of the present application;

[0036] Figure 5 This is a SEM image of the powder prepared in Comparative Example 2 of the present application;

[0037] Figure 6 This is a SEM image of the powder prepared in Comparative Example 3 of the present application;

[0038] Figure 7 This is a SEM image of the powder prepared in Comparative Example 4 of the present application;

[0039] Figure 8 This is a SEM image of the powder prepared in Comparative Example 5 of the present application;

[0040] Fig. 9 Schematic diagram of the structure of the target material prepared by Example 1 of the present application;

[0041] Fig.10 This is a schematic diagram of the structure of the target material after coating prepared in Example 1 of the present application;

[0042] Fig.11 This is a microscope image of the target coating structure prepared by Example 1 of the present application.

[0043] Fig.12 This is a structural diagram of the target coating thickness prepared by Example 1 of the present application. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments and drawings. The specific embodiments described herein are only used to explain the present invention and are not intended to constitute any limitation to the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concepts of the present disclosure. Such structures and technologies are also described in many publications.

[0045] The aluminum-doped zinc oxide nanopowder of the present invention is a solid sphere, the D50 of the nanopowder is 10-30um, and the density of the nanopowder is 1.2-1.4g / cm 3 .

[0046] The raw materials for preparing the nanopowder of the present invention include zinc oxide and aluminum oxide, and as a preferred embodiment, further include a dispersant, a binder and a defoaming agent; preferably, the dispersant is selected from water and / or SD-3 organic bentonite dispersant, the binder is PVA glue, and the defoaming agent is n-butanol.

[0047] The particle size of zinc oxide used in the embodiment of the present application is 1 um, the particle size of aluminum oxide is 1 um, and the water used in the embodiment of the present application is deionized water.

[0048] Example 1

[0049] A method for preparing aluminum-doped zinc oxide nanopowder comprises the following steps:

[0050] (1) 19.6 kg of zinc oxide, 0.4 kg of aluminum oxide, 150 g of SD-3 organic bentonite dispersant and 8.5 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0051] (2) mixing the mixture obtained in step (1) with 1800 g of a binder to obtain a slurry having a pH of 8;

[0052] (3) The slurry obtained in step (2) is subjected to centrifugal spray drying, the air inlet temperature of the centrifugal spray drying is 260° C., the atomization frequency of the centrifugal spray drying is 300 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained.

[0053] The distribution of the powder D50 prepared in this example is as follows Figure 1 As shown in the figure, it can be seen that the particle size distribution is relatively uniform.

[0054] The SEM image of the powder prepared in this example is as follows Figure 2 and Figure 3 As shown, from Figure 2 and Figure 3 It can be seen that the powder particle size distribution is uniform and the size is relatively uniform, and the powder is solid powder.

[0055] Example 2

[0056] A method for preparing aluminum-doped zinc oxide nanopowder comprises the following steps:

[0057] (1) 19.6 kg of zinc oxide, 0.4 kg of aluminum oxide, 150 g of SD-3 organic bentonite dispersant and 8.5 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0058] (2) mixing the mixture obtained in step (1) with 3600 g of a binder to obtain a slurry having a pH of 8.5;

[0059] (3) The slurry obtained in step (2) is subjected to centrifugal spray drying, the air inlet temperature of the centrifugal spray drying is 260° C., the atomization frequency of the centrifugal spray drying is 300 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained.

[0060] Comparative Example 1

[0061] A method for preparing aluminum-doped zinc oxide nanopowder comprises the following steps:

[0062] (1) 19.6 kg of zinc oxide, 0.4 kg of aluminum oxide, 450 g of SD-3 organic bentonite dispersant and 17 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0063] (2) mixing the mixture obtained in step (1) with 1800 g of a binder to obtain a slurry having a pH of 9.5;

[0064] (3) The slurry obtained in step (2) is subjected to centrifugal spray drying, the air inlet temperature of the centrifugal spray drying is 260° C., the atomization frequency of the centrifugal spray drying is 300 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained.

[0065] The SEM image of the powder obtained in this comparative example is as follows: Figure 4 As shown, from Figure 4 It can be seen that the powder obtained in this comparative example is a hollow spherical shell.

[0066] Comparative Example 2

[0067] A method for preparing aluminum-doped zinc oxide nanopowder comprises the following steps:

[0068] (1) 19.6 kg of zinc oxide, 0.4 kg of aluminum oxide, 450 g of SD-3 organic bentonite dispersant and 17 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0069] (2) mixing the mixture obtained in step (1) with 1800 g of a binder to obtain a slurry having a pH of 9.5;

[0070] (3) The slurry obtained in step (2) is subjected to centrifugal spray drying, the air inlet temperature of the centrifugal spray drying is 200° C., the atomization frequency of the centrifugal spray drying is 300 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained.

[0071] The SEM image of the powder obtained in this comparative example is as follows: Figure 5 As shown, from Figure 5 It can be seen that the powder obtained in this comparative example is a hollow spherical shell.

[0072] Comparative Example 3

[0073] A method for preparing aluminum-doped zinc oxide nanopowder comprises the following steps:

[0074] (1) 19.6 kg of zinc oxide, 0.4 kg of aluminum oxide, 450 g of SD-3 organic bentonite dispersant and 17 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0075] (2) mixing the mixture obtained in step (1) with 1800 g of a binder to obtain a slurry having a pH of 9;

[0076] (3) The slurry obtained in step (2) is subjected to centrifugal spray drying, the air inlet temperature of the centrifugal spray drying is 150° C., the atomization frequency of the centrifugal spray drying is 300 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained.

[0077] The SEM image of the powder obtained in this comparative example is as follows: Figure 6 As shown, from Figure 6 It can be seen that the powder obtained in this comparative example is a hollow spherical shell.

[0078] Comparative Example 4

[0079] A method for preparing aluminum-doped zinc oxide nanopowder comprises the following steps:

[0080] (1) 19.6 kg of zinc oxide, 0.4 kg of aluminum oxide, 450 g of SD-3 organic bentonite dispersant and 17 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0081] (2) mixing the mixture obtained in step (1) with 1800 g of a binder to obtain a slurry having a pH of 9;

[0082] (3) The slurry obtained in step (2) is subjected to centrifugal spray drying, the air inlet temperature of the centrifugal spray drying is 260° C., the atomization frequency of the centrifugal spray drying is 300 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained.

[0083] Comparative Example 5

[0084] A method for preparing aluminum-doped zinc oxide nanopowder comprises the following steps:

[0085] (1) 19.6 kg of zinc oxide, 0.4 kg of aluminum oxide, 450 g of SD-3 organic bentonite dispersant and 8.5 g of defoaming agent n-butanol were mixed and ground, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the mixture was ground for 20 h to obtain a mixture;

[0086] (2) mixing the mixture obtained in step (1) with 1800 g of a binder to obtain a slurry having a pH of 8.5;

[0087] (3) The slurry obtained in step (2) is subjected to centrifugal spray drying, the air inlet temperature of the centrifugal spray drying is 260° C., the atomization frequency of the centrifugal spray drying is 300 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained.

[0088] Comparative Example 6

[0089] The difference between Comparative Example 6 and Example 1 is that the atomization frequency of centrifugal spray drying in the powder preparation process of Comparative Example 6 is 200 Hz.

[0090] Specifically:

[0091] A method for preparing aluminum-doped zinc oxide nanopowder comprises the following steps:

[0092] (1) 19.6 kg of zinc oxide, 0.4 kg of aluminum oxide, 150 g of SD-3 organic bentonite dispersant and 8.5 g of defoaming agent n-butanol were mixed and ground, the grinding solvent used for grinding was 19 L of water, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the grinding was performed for 20 h to obtain a mixed powder with a particle size of 500-600 nm;

[0093] (2) placing the mixed powder obtained in step (1) into a degumming furnace, heating and keeping the mixture at a heating temperature of 450° C. for 3 days, and allowing the mixture to cool naturally to room temperature to obtain a degummed mixed powder, and mixing the degummed mixed powder with 1800 g of a binder to obtain a slurry with a pH of 8;

[0094] (3) The slurry obtained in step (2) is subjected to centrifugal spray drying, the air inlet temperature of the centrifugal spray drying is 260° C., the atomization frequency of the centrifugal spray drying is 200 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained.

[0095] The SEM image of the powder obtained in this comparative example is as follows: Figure 7 As shown, from Figure 7 It can be seen that the powder obtained in this comparative example is a hollow spherical shell.

[0096] Comparative Example 7

[0097] The difference between Comparative Example 7 and Example 1 is that the atomization frequency of centrifugal spray drying in the powder preparation process of Comparative Example 7 is 400 Hz.

[0098] Specifically:

[0099] A method for preparing aluminum-doped zinc oxide nanopowder comprises the following steps:

[0100] (1) 19.6 kg of zinc oxide, 0.4 kg of aluminum oxide, 150 g of SD-3 organic bentonite dispersant and 8.5 g of defoaming agent n-butanol were mixed and ground, the grinding solvent used for grinding was 19 L of water, the grinding medium used was zirconium oxide with a particle size of 3 mm, the grinding speed was 30 r / min, and the grinding was performed for 20 h to obtain a mixed powder with a particle size of 500-600 nm;

[0101] (2) placing the mixed powder obtained in step (1) into a degumming furnace, heating and keeping the mixture at a heating temperature of 450° C. for 3 days, and allowing the mixture to cool naturally to room temperature to obtain a degummed mixed powder, and mixing the degummed mixed powder with 1800 g of a binder to obtain a slurry with a pH of 8;

[0102] (3) The slurry obtained in step (2) is subjected to centrifugal spray drying, the air inlet temperature of the centrifugal spray drying is 260° C., the atomization frequency of the centrifugal spray drying is 400 Hz, and after drying, the aluminum-doped zinc oxide nanopowder is obtained.

[0103] The SEM image of the powder obtained in this comparative example is as follows: Figure 8 As shown, from Figure 8 It can be seen that the powder obtained in this comparative example is a hollow spherical shell.

[0104] The aluminum-doped zinc oxide nanopowder prepared in Example 1 was pressed into shape by cold isostatic pressing at a pressure of 225 MPa for 15 min to obtain a rectangular blank, which was placed in a degumming furnace for heating and degumming at a temperature of 450° C. for 3 days and then naturally cooled to room temperature. The blank was then buried in thermal conductive sand (silicon dioxide quartz sand) and sintered at a temperature of 1550° C. for 6 days to obtain an aluminum-doped zinc oxide target.

[0105] The structure of the target material is as follows Fig. 9 As shown, from Fig. 9 It can be seen that the zinc oxide nanopowder described in this application can be used to prepare a target material with a size of 10 inches.

[0106] The target material prepared above is coated, such as Fig.10 As shown, from Fig.10 It can be seen that there is no cracking and delamination, and its microscope image (such as Fig.11) shows excellent surface uniformity, with a thickness of up to 882nm (as shown Fig.12 shown).

[0107] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. An aluminum-doped zinc oxide nanopowder, It is characterized in that The nano powder is a solid powder, the D50 of the nano powder is 10-30um, and the density of the nano powder is 1.2-1.4g / cm 3 .

2. The nanopowder according to claim 1, It is characterized in that The raw materials for preparing the nano powder include zinc oxide and aluminum oxide; Preferably, the raw materials for preparing the nanopowder further include a dispersant, a binder and a defoaming agent; Preferably, the dispersant is selected from water and / or SD-3 organobentonite dispersant; preferably, the water is deionized water; Preferably, the adhesive is PVA glue Preferably, the degassing agent is n-butanol.

3. The nanopowder according to claim 1, It is characterized in that The weight ratio of zinc oxide to aluminum oxide in the raw materials for preparing the nanopowder is (95-99.5):(5-0.5); Preferably, the weight ratio of the dispersant, binder, defoaming agent and alumina in the raw materials for preparing the nanopowder is (0.3-1.1):(2-9):(0.02-0.04):1, preferably 0.38:9:0.02:1, and more preferably 0.38:4.5:0.02:

1.

4. The method for preparing the nanopowder according to any one of claims 1 to 3, The following steps are involved: (1) mixing zinc oxide, aluminum oxide, a dispersant and a defoaming agent and grinding them to obtain a mixture; (2) mixing the mixture obtained in step (1) with a binder to obtain a slurry; (3) Drying and granulating the slurry obtained in step (2) to obtain the aluminum-doped zinc oxide nanopowder.

5. The preparation method according to claim 4, It is characterized in that In step (1), the particle size of the zinc oxide is 0.8-1.2 um, and the particle size of the aluminum oxide is 0.8-1.2 um.

6. The preparation method according to claim 4 or 5, It is characterized in that The grinding medium used in the grinding is zirconium oxide; Preferably, the particle size of the zirconium oxide is 2-3 mm, preferably 3 mm; Preferably, the grinding speed is 30-50r / min; Preferably, the grinding time is 20-28 hours.

7. The preparation method according to claim 4, It is characterized in that The pH of the slurry is 8-9.

5.

8. The preparation method according to claim 4, It is characterized in that In step (3), the drying is centrifugal spray drying; Preferably, the inlet air temperature of the centrifugal spray drying is 150-300°C, preferably 260°C; Preferably, the atomization frequency of the centrifugal spray drying is 250-350 Hz.

9. Use of the aluminum-doped zinc oxide nanopowder according to any one of claims 1 to 3 or the aluminum-doped zinc oxide nanopowder obtained by the preparation method according to any one of claims 4 to 8 in piezoelectric film magnetron sputtering targets.

10. The use according to claim 9, It is characterized in that The size of the piezoelectric film magnetron sputtering target is 250-260 mm.