Glass-compounded sodium bismuth titanate-based high-temperature energy storage ceramic material as well as preparation method and application thereof

Through the high-temperature energy storage ceramic material of bismuth titanate composite with glass, the problem of degradation of energy storage performance of dielectric ceramic materials in high temperature environments is solved, and the stability and efficient energy storage density in aerospace and other fields are achieved, simplifying the The process and reduce costs.

CN118908724APending Publication Date: 2024-11-08SHAANXI UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410960679.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The energy storage performance of existing dielectric ceramic materials has decreased in high temperature environments, making it difficult to achieve stability and large-scale production, and the process is complex and costly, which limits its application in aerospace and other fields.

Method used

Using a sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass, molten glass powder 40Na2O-18CaO-42SiO2 and calcined powder 0.85 (Na0.5Bi0.5) 0.75Sr0.25TiO3-0.15Ca(Mg1/3Ta2 /3)O3 compound sintering to form a composite material with excellent high-temperature energy storage performance.

Benefits of technology

Maintain excellent energy storage stability within a wide temperature range of 30-130℃, the energy storage density reaches 5.5J/cm3, and the energy storage efficiency is as high as 92.0%, which significantly improves the mechanical and electrical properties of the material and reduces production costs. Have the potential for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908724A_ABST
    Figure CN118908724A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium bismuth titanate-based high-temperature energy storage ceramic material compounded with glass as well as a preparation method and application of the sodium bismuth titanate-based high-temperature energy storage ceramic material. According to the sodium bismuth titanate-based high-temperature energy storage ceramic material, molten glass powder 40Na2O-18CaO-42SiO2 and calcined powder 0.85 (Na < 0.5 > Bi < 0.5 >) < 0.75 > Sr < 0.25 > TiO < 3 >-0.15 Ca (Mg < 1 / 3 > Ta < 2 / 3 >) O3 are compounded to form a composite material with excellent high-temperature energy storage performance. 40Na2O-18CaO-42SiO2 glass is introduced as a liquid-phase sintering aid, so that the sintering temperature is effectively reduced, grain refinement is promoted, the structure of the ceramic material is more compact, the mechanical property and the electrical property are remarkably improved, meanwhile, formation of an electric breakdown path can be effectively dispersed and hindered, and the breakdown strength of the ceramic material is remarkably improved. The ceramic material is cheap in raw material, simple in preparation process, short in production period and suitable for batch production, can meet the strict requirements of a high-pulse power system, improves the stability and reliability of the system, and can also be applied to other fields needing high energy storage density and good high-temperature stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technology of preparing lead-free energy storage ceramic materials, and in particular relates to a sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass, and a preparation method and application thereof. Background Art

[0002] With the booming development of pulse power technology, its application in aerospace, oil exploration, power vehicles and other fields is becoming more and more extensive. However, high temperature failure has become a major obstacle in the practical application of these fields. Especially in harsh environments such as aerospace, electronic control devices are often located near the engine, and the operating temperature can be as high as 200℃ to 300℃, which puts extremely high demands on the high temperature resistance and stability of capacitors.

[0003] Dielectric ceramic materials have attracted widespread attention due to their high power density and fast charge and discharge rates. However, despite these advantages, the energy storage performance of dielectric ceramic materials will significantly decrease in high temperature environments, leading to capacitor failure. In addition, high temperatures may also cause physical and chemical changes inside the material, such as thermal expansion and contraction, insulation medium failure, etc., further affecting the performance of the capacitor, thus limiting its widespread use in practical applications.

[0004] In order to overcome the performance limitations of dielectric ceramic materials at high temperatures, there are currently a variety of methods to optimize the high-temperature energy storage performance of dielectric ceramic materials, mainly ion doping, component solid solution and improved sintering process, but there are still many problems. Ion doping changes the microstructure and electrical properties of the material by introducing specific ions. However, the energy storage performance of the dielectric ceramic material obtained by this method at high temperatures is limited, and the selection of doping ions and the control of doping amounts require precise regulation, the process is complex and the cost is high; component solid solution improves the comprehensive performance of the material by mixing different components to form a solid solution, but this method also faces the challenges of expensive raw materials and complex preparation processes, and it is difficult to achieve large-scale production; improving the sintering process can improve the density and microstructure of the material, but for high-temperature stable capacitor materials, it is often difficult to achieve ideal high-temperature energy storage performance only by optimizing the sintering process.

[0005] Therefore, the degree of optimization of the energy storage performance of existing dielectric ceramic materials at high temperatures is limited, and the raw materials are expensive and the preparation process is complicated, making it difficult to achieve large-scale production, which limits the application of dielectric ceramic materials in the field of high-temperature energy storage. How to prepare high-temperature stable capacitor materials with stable performance and controllable costs, how to further improve the energy storage density and efficiency of capacitors while ensuring high-temperature stability, and meet the stability and reliability in high-temperature environments, these are all problems that need to be urgently solved for high-temperature stable capacitor materials. Summary of the invention

[0006] In view of the special requirements for capacitor materials in extreme high temperature environments such as aerospace, oil exploration and power vehicles, the existing dielectric ceramic materials are limited in the degree of optimization of energy storage performance under extreme high temperatures, and it is impossible to further improve the energy storage density and efficiency of capacitors while ensuring high temperature stability. The present invention aims to provide a sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass, and a preparation method and application thereof.

[0007] To achieve the above object, the present invention is implemented through the following technical solutions:

[0008] The present invention provides a sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass, wherein the sodium bismuth titanate-based high-temperature energy storage ceramic material has a chemical formula of 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-xwt%(40Na2O-18CaO-42SiO2), where 1.0≤x≤12.0;

[0009] The sodium bismuth titanate-based high-temperature energy storage ceramic material is prepared by mixing molten glass powder 40Na2O-18CaO-42SiO2 with calcined powder 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3 composite sintering is obtained.

[0010] Furthermore, 3.0≤x≤9.0.

[0011] Furthermore, the x=6.0.

[0012] The present invention provides a method for preparing the above-mentioned sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass, comprising:

[0013] S1, weigh Na2CO3, Bi2O3, SrCO3, TiO2, CaCO3, MgO and Ta2O5 according to the proportion, mix and ball-mill, then dry, calcine at 800-900℃ for 1-3h, crush, grind and sieve to obtain calcined powder;

[0014] S2, weighing Na2O, CaO and SiO2 according to the chemical formula, mixing and ball-milling, drying, melting at 1400-1500°C for 1-2h, annealing, crushing, grinding and sieving to obtain molten glass powder;

[0015] S3, adding 1% to 12% by mass of the molten glass powder obtained in step S2 to the calcined powder obtained in step S1, mixing by ball milling, drying, crushing, grinding, screening, pressing into a green body, sintering at 1100 to 1200° C. for 3 to 5 hours, and obtaining a sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass.

[0016] In step S1, the temperature is raised from room temperature to 800-900° C. at a rate of 5° C. / min, and after calcination, the temperature is lowered to 500° C. at a rate of 5° C. / min, and then cooled to room temperature in the furnace.

[0017] The annealing temperature in step S2 is 500° C. to 600° C., and the annealing time is 5 hours.

[0018] In the step S3, the sintering temperature is 1140° C. to 1180° C., and the holding time is 4 hours.

[0019] In the steps S1, S2 and S3, the mass ratio of material: ball: water in ball milling is 1:2:2, and the ball milling time is 10 hours.

[0020] The sintering system in step 3 is: heating from room temperature to 1100° C. to 1200° C. at 5° C. / min, cooling to 500° C. at 5° C. / min after sintering, and then cooling to room temperature in the furnace.

[0021] The present invention provides an application of the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass in a high-temperature energy storage device.

[0022] Compared with the prior art, the present invention has the following beneficial results:

[0023] The sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass provided by the present invention comprises a molten glass powder 40Na2O-18CaO-42SiO2 and a calcined powder 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3, the two are combined to form a composite material with excellent high-temperature energy storage performance; due to the low and stable dielectric constant of 40Na2O-18CaO-42SiO2 glass, the ceramic material finally obtained can still maintain stable energy storage performance in a high-temperature environment; at the same time, the glass phase can effectively disperse and hinder the formation of electrical breakdown paths, thereby improving the overall electrical breakdown resistance of the ceramic material; when the addition of 40Na2O-18CaO-42SiO2 glass is 6%, the obtained sodium bismuth titanate-based high-temperature energy storage ceramic material maintains excellent energy storage stability in a wide temperature range of 30 to 130°C, and the energy storage density reaches 5.5J / cm 3The energy storage efficiency is as high as 92.0%, far exceeding that of traditional ceramic materials. It can meet the stringent requirements of high-pulse power systems, improve the stability and reliability of the system, and can also be used in other fields that require high energy storage density and good high-temperature stability.

[0024] The preparation method of the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass provided by the present invention simplifies the raw material formula and preparation process of the ceramic material by using a multi-material mixing technology, and effectively reduces the sintering temperature and promotes grain refinement by introducing 40Na2O-18CaO-42SiO2 glass as a liquid phase sintering aid, making the structure of the ceramic material denser, thereby improving its mechanical and electrical properties, and significantly improving the breakdown strength (E b ), which not only saves energy but also reduces material defects generated during high-temperature sintering; the materials used in the entire preparation process of the present invention meet environmental protection requirements, have no harmful substance emissions, have simple processing methods and low prices, and significantly reduce production costs. The selected materials and processes have the potential for large-scale production, which is helpful to promote the commercialization of energy storage ceramic materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A comparison diagram of energy storage performance of different ceramic materials of the present invention;

[0026] Figure 2 XRD diagrams of different ceramic materials of the present invention, wherein (a) is an XRD diagram of different ceramic materials, (b) is an XRD diagram of 40Na2O-18CaO-42SiO2 glass of the present invention, and (c) is an XRD diagram of the ceramic sample of comparative example 2;

[0027] Figure 3 The SEM images and grain size distribution diagrams of different ceramic materials of the present invention, wherein (a) is the SEM image and particle size distribution of the ceramic sample of Comparative Example 1, (b) is the SEM image and particle size distribution of the ceramic sample of Example 3, (c) is the SEM image and particle size distribution of the ceramic sample of Example 1, (d) is the SEM image and particle size distribution of the ceramic sample of Example 4, (e) is the SEM image and particle size distribution of the ceramic sample of Example 5, and (f) is a comparison diagram of the average particle sizes of different samples;

[0028] Figure 4 Different ceramic materials ε r and tanδ versus temperature, wherein (a) is a dielectric temperature diagram of the ceramic samples of Examples 1-5 and Comparative Example 1, and (b) is a dielectric temperature diagram of the ceramic sample of Comparative Example 2;

[0029] Figure 5Figures showing the change of polarization intensity with electric field for different ceramic materials of the present invention, wherein (a) is a graph showing the change of polarization intensity with electric field under breakdown electric field, (b) is a graph showing the change of polarization intensity with electric field under 80 kV / cm, and (c) is a graph showing the comparison of ferroelectric properties between Example 1 and Comparative Example 2;

[0030] Figure 6 The graphs are as follows: (a) is a graph showing how polarization intensity varies with electric field at different temperatures and frequencies for the ceramic sample of Example 3 of the present invention; (b) is a graph showing how energy storage performance varies with temperature; (c) is a graph showing how polarization intensity varies with electric field at different frequencies; and (d) is a graph showing how energy storage performance varies with frequency. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0032] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0033] If no specific experimental steps or conditions are specified in the examples, the experiments can be carried out according to the conventional experimental steps or conditions described in the literature in the art. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0034] Example 1: Sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass

[0035] This embodiment provides a sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass. The stoichiometric formula of the sodium bismuth titanate-based high-temperature energy storage ceramic material is 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-6.0wt% (40Na2O-18CaO-42SiO2).

[0036] The specific preparation steps include:

[0037] Step 1: Prepare 0.85(Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg1 / 3 Ta 2 / 3 )O3 calcined powder

[0038] 1.681g Na2CO3, 7.396g Bi2O3, 3.146g SrCO3, 6.877g TiO2, 1.506g CaCO3, 0.201g MgO and 2.194g Ta2O5 were weighed in each ball mill, mixed with zirconium ball stone and deionized water in a mass ratio of 1:2:2, and ball milled for 10h; after ball milling, dried at 85℃ for 48h, and calcined at 875℃ for 2h After sintering, the mixture was crushed and ground through a 120-mesh sieve to obtain 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3 calcined powder.

[0039] Step 2: Preparation of 40Na2O-18CaO-42SiO2 molten glass powder

[0040] According to the chemical formula 40Na2O-18CaO-42SiO2, 14.790g of Na2CO3, 6.336g of CaCO3 and 8.874g of SiO2 were weighed, and the powders were mixed with zirconium spheroids and deionized water in a mass ratio of 1:2:2, and placed in a ball mill for 10 hours. After ball milling, the mixture was dried at 85°C for 48 hours, melted at 1450°C for 1 hour, poured into a mold preheated to 200°C, and after forming, it was transferred to an annealing furnace at 600°C and kept warm for 5 hours. After cooling with the furnace, a glass sample was obtained, which was crushed and ground and passed through a 120-mesh sieve to obtain 40Na2O-18CaO-42SiO2 molten glass powder;

[0041] Step 3: Preparation of 0.85(Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-6.0wt%(40Na2O-18CaO-42SiO 2) ceramics

[0042] Weigh 20g of the calcined powder obtained in step 1 and 1.2g of the molten glass powder obtained in step 2 respectively, ball mill them with zirconium spheroids and deionized water in a mass ratio of 1:2:2 for 10h, and dry them at 85°C for 48h after ball milling; crush and grind them and pass them through a 120-mesh sieve to obtain a mixed powder, weigh 0.35g of the mixed powder and press it by cold isostatic pressing (pressing process parameters: 200MPa holding pressure for 3min, 190MPa holding pressure for 5min, 40MPa / min pressure relief), and sinter at 1140°C for 4h (sintering system is: ) to obtain 0.85(Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-6.0wt%(40Na2O-18CaO-42SiO 2) ceramics.

[0043] Example 2: Preparation of sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass

[0044] This embodiment provides a method for preparing a sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass on the basis of embodiment 1. The chemical formula of the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass is 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-1.0wt%(40Na2O-18CaO-42SiO2). The remaining steps are the same as in Example 1.

[0045] Weigh 20g of the calcined powder from step 1 and 0.2g of the molten glass powder from step 2 respectively and sinter them;

[0046] 0.85(Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-1.0wt%(40Na2O-18CaO-42SiO 2) ceramics.

[0047] Example 3: Preparation of sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass

[0048] This embodiment provides a method for preparing a sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass on the basis of embodiment 1. The chemical formula of the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass is 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-3.0wt%(40Na2O-18CaO-42SiO2). The remaining steps are the same as in Example 1.

[0049] Weigh 20g of the calcined powder from step 1 and 0.6g of the molten glass powder from step 2 and sinter them to obtain 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-3.0wt%(40Na2O-18CaO-42SiO 2) ceramics.

[0050] Example 4: Preparation of sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass

[0051] This embodiment provides a method for preparing a sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass on the basis of embodiment 1. The chemical formula of the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass is 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-9.0wt%(40Na2O-18CaO-42SiO2). The remaining steps are the same as in Example 1.

[0052] Weigh 20g of the calcined powder from step 1 and 1.8g of the molten glass powder from step 2 and sinter them to obtain 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-9.0wt%(40Na2O-18CaO-42SiO 2) ceramics.

[0053] Example 5: Preparation of sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass

[0054] This embodiment provides a method for preparing a sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass on the basis of embodiment 1. The chemical formula of the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass is 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-12.0wt%(40Na2O-18CaO-42SiO2). The remaining steps are the same as in Example 1.

[0055] Weigh 20g of the calcined powder from step 1 and 2.4g of the molten glass powder from step 2 and sinter them to obtain 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3-12.0wt%(40Na2O-18CaO-42SiO 2) ceramics.

[0056] Comparative Example 1:

[0057] The preparation method of Example 1 was adopted, and the 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3 powder was pressed by cold isostatic pressing (pressing process parameters: 200MPa holding pressure for 3min, 190MPa holding pressure for 5min, 40MPa / min pressure release), and sintered at 1140℃ for 4h (sintering system: ) to obtain 0.85(Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3 ceramic samples.

[0058] Comparative Example 2:

[0059] The raw materials for the 40Na2O-18CaO-42SiO2 molten glass powder were directly doped without melting the 40Na2O-18CaO-42SiO2 glass powder for process comparison. The raw materials for the 40Na2O-18CaO-42SiO2 molten glass powder (0.887 g Na2CO3, 0.380 g CaCO3 and 0.532 g SiO2) were weighed and mixed with the raw materials for the 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3 powder raw materials (1.461g Na2CO3, 6.431g Bi2O3, 2.736g SrCO3, 5.980g TiO2, 1.309g CaCO3, 0.174g MgO and 1.098g Ta2O5). The preparation method of Example 1 is adopted to directly mix and ball-mill the above raw materials, and step 2 is discarded. The powder synthesized in step 1 is directly subjected to the operation in step 3 without adding molten glass powder. Finally, the obtained powder is pressed by cold isostatic pressing (pressing process parameters: 200MPa pressure for 3min, 190MPa pressure for 5min, 40MPa / min pressure release), and sintered at 1140℃ for 4h (sintering system is: ) to obtain 0.85(Na 0.5+6.0wt% Bi 0.5 ) 0.75 Sr 0.25 TiO3-0.15Ca 1+6.0wt% (Mg 1 / 3 Ta 2 / 3 )O3-6.0wt%SiO2 ceramic sample.

[0060] Example 6: Performance Test

[0061] The ceramic samples obtained in Examples 1 to 5 and the comparative example were polished and cleaned, and silver electrode slurry was evenly coated on both sides of the samples. The samples coated with silver electrodes were placed in an alumina sagger with zirconium oxide as a backing plate, and then the alumina sagger was placed in a box furnace and sintered at 600°C for 20 minutes to obtain various test samples. The energy storage performance and crystal structure of different samples were tested respectively. The specific results are shown in the attached Figure 1-6 shown.

[0062] By the attached Figure 1 The data show that the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass provided by the present invention has certain advantages in energy storage performance compared with other lead-free energy storage ceramic materials. It obtains an energy storage efficiency of 92.0% and an energy storage capacity of 5.49 J / cm2 at a breakdown electric field of 320 kV / cm2.3 The energy storage density and energy storage performance are better than other lead-free energy storage ceramic materials.

[0063] By the attached Figure 2 The data shows that Figure 2 In the figure, (a) is a comparison of XRD patterns of different samples, (b) is an XRD pattern of 40Na2O-18CaO-42SiO2 molten glass powder, and (c) is an XRD pattern of the ceramic sample of Comparative Example 2. The XRD pattern of 40Na2O-18CaO-42SiO2 glass has typical amorphous phase characteristics. After the glass modification of the amorphous phase, the ceramic sample retains the original second phase, which indicates that the incorporation of 40Na2O-18CaO-42SiO2 glass does not affect the multiphase structure of the ceramic matrix. Therefore, there is ion interdiffusion between the molten amorphous phase and the ceramic matrix, rather than a chemical reaction between the two materials. At the same time, the ceramic sample in Comparative Example 1 also retains the original second phase and forms a solid solution.

[0064] By the attached Figure 3 The data shows that Figure 3 In the figure, (a) is the SEM image and particle size distribution of the ceramic sample of comparative example 1, (b) is the SEM image and particle size distribution of the ceramic sample of embodiment 3, (c) is the SEM image and particle size distribution of the ceramic sample of embodiment 1, (d) is the SEM image and particle size distribution of the ceramic sample of embodiment 4, (e) is the SEM image and particle size distribution of the ceramic sample of embodiment 5, and (f) is a comparison of the average particle sizes of different samples. All sample ceramics have a dense microstructure, almost no pores, and show good crystallization properties. At the same time, there are a small amount of lamellar grains in the micromorphology of each component, which is a typical micromorphology of the second phase in the ceramic sample, which is consistent with the XRD results. After the glass is modified, the signs of liquid phase sintering are very obvious. The 40Na2O-18CaO-42SiO2 glass transforms into liquid phase during the sintering process and accumulates at the grain boundaries. Because 40Na2O-18CaO-42SiO2 glass has a lower diffusion rate and softening point, it forms a liquid phase and wets the grains during the sintering stage, thereby promoting the mass transfer process. As the sintering temperature decreases, the average grain size decreases from 1.30μm to 1.17μm, indicating that 40Na2O-18CaO-42SiO2 glass can inhibit grain growth; at the same time, the rich amorphous phase at the grain boundary reduces the generation of pores and increases the density of the ceramic. According to the empirical formula The reduced grain size and dense microstructure are beneficial to improving the breakdown strength (E b ).

[0065] Further analysis of the dielectric properties of different samples was carried out by Figure 4 The data shows that Figure 4In the figure, (a) is the dielectric temperature diagram of the ceramic samples of Examples 1-5 and Comparative Example 1, and (b) is the dielectric temperature diagram of the ceramic sample of Comparative Example 2. As the content of 40Na2O-18CaO-42SiO2 glass increases, the maximum dielectric constant (ε m ) gradually decreases, the dielectric peak tends to be flat, and the dielectric constant (ε r ) shows strong thermal stability. The lower ε r It is beneficial to prolong the saturation polarization, thus obtaining better energy storage performance under higher electric fields; on the other hand, due to ε r The value is small but stable with temperature changes, which can inhibit the attenuation of polarization intensity at high temperature, thereby maintaining a stable polarization response and energy storage performance in a larger temperature range. Comparing the tanδ of different ceramic samples, it decreases with the increase of the amount of glass introduced, which shows that the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass provided by the present invention has practical application potential in the field of energy storage, especially under high temperature conditions. When the process of composite glass and ceramic in the present invention is not adopted, the dielectric constant of the ceramic sample in Comparative Example 2 is relatively high, which is not conducive to prolonging the saturation polarization; at the same time, tanδ is also slightly increased, which is not conducive to actual energy storage applications.

[0066] By the attached Figure 5 The data show that the ferroelectric properties of different samples are analyzed. Figure 5 In the figure, (a) is the variation of polarization intensity with electric field under breakdown electric field, (b) is the variation of polarization intensity with electric field under 80 kV / cm, and (c) is the comparison of ferroelectric properties between Example 1 and Comparative Example 2. 0.5 Bi 0.5 ) 0.75 Sr 0.25 Compared with TiO3 ceramic samples, the addition of 40Na2O-18CaO-42SiO2 glass improves the breakdown strength of ceramics. This is due to the ε r The value is small but stable with temperature changes, thereby delaying polarization saturation and increasing the breakdown strength to 320kV / cm. When traditional doping methods are adopted, excessive ion doping leads to the deterioration of breakdown strength. The ceramic sample of Comparative Example 2 shows the phenomenon of incompatibility between doped ions and ceramic matrix. It is necessary to optimize the energy storage performance of ceramic samples by further improving the doping concentration and the screening of doping ions, which is costly and has a long process cycle, and is not conducive to large-scale application. After adopting the multi-material mixing technology of the present invention, when x=3.0 and 6.0 (for Example 3 and Example 1, respectively), the ceramic samples obtained 5.2J / cm at 280kV / cm and 320kV / cm, respectively. 3 energy storage density, 92.2% energy storage efficiency and 5.5J / cm 3The energy storage density of 92.0% and the energy storage efficiency can be respectively applied to the application scenarios of low electric fields (E < 300 kV / cm) and medium electric fields (300 kV / cm < E < 500 kV / cm).

[0067] For dielectric ceramic capacitors applied in various environments, the temperature and frequency stability of their energy storage performance are crucial. Analyze the hysteresis loops of the ceramic samples of the third embodiment at different temperatures and frequencies. From the attached Figure 6 data, it can be seen that in the attached Figure 6 , (a) is the graph of polarization intensity versus electric field at different temperatures, (b) is the graph of energy storage performance versus temperature, (c) is the graph of polarization intensity versus electric field at different frequencies, and (d) is the graph of energy storage performance versus frequency. In the temperature range of 30 °C to 130 °C, the energy storage density of the ceramic samples is stable at 1.59 - 1.74 J / cm 3 , and the energy storage efficiency is stable at 91.1% - 92.0%. In extreme environments, not only excellent temperature stability is required, but frequency stability is also crucial. The hysteresis loops of the ceramic samples do not change significantly with frequency, and there are no obvious fluctuations in the energy storage density and energy storage efficiency, verifying the frequency stability of the energy storage performance of the ceramic samples. In summary, 0.85(Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO3 - 0.15Ca(Mg 1 / 3 Ta 2 / 3 )O3 - 6.0 wt% (40Na2O - 18CaO - 42SiO 2) The ceramic samples have excellent temperature and frequency stability and are expected to replace lead-based ceramics as the dielectric material for high-temperature pulsed power capacitors.

[0068] The above content is only to illustrate the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any modification made on the basis of the technical solution according to the technical idea proposed by the present invention falls within the protection scope of the claims of the present invention.

Claims

1. A sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass, It is characterized in that The chemical formula of the sodium bismuth titanate-based high-temperature energy storage ceramic material is 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO 3 -0.15Ca(Mg 1 / 3 Ta 2 / 3 ) 3 -x wt%(40Na 2 O-18CaO-42SiO 2 ), where 1.0≤x≤12.0; The sodium bismuth titanate-based high-temperature energy storage ceramic material is prepared by melting 40 Na 2 O-18CaO-42SiO 2 With calcined powder 0.85 (Na 0.5 Bi 0.5 ) 0.75 Sr 0.25 TiO 3 -0.15Ca(Mg 1 / 3 Ta 2 / 3 ) 3 Obtained by compound sintering.

2. According to claim 1, the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass, It is characterized in that Said 3.0≤x≤9.

0.

3. According to claim 2, the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass, It is characterized in that Said x=6.

0.

4. A method for preparing the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass as claimed in any one of claims 1 to 3, It is characterized in that include: S1, weigh Na according to the proportion 2 CO 3 、Bi 2 O 3 、SrCO 3 、TiO 2 、CaCO 3 , MgO and Ta 2 O 5 , after mixing and ball milling, drying, calcining at 800-900°C for 1-3h, crushing, grinding and sieving to obtain calcined powder; S2, weigh Na according to the chemical formula 2 O, CaO and SiO 2 The mixed materials are ball-milled and then dried, melted at 1400-1500°C for 1-2h, annealed, crushed, ground and sieved to obtain molten glass powder; S3, adding 1% to 12% by mass of the molten glass powder obtained in step S2 to the calcined powder obtained in step S1, mixing by ball milling, drying, crushing, grinding, screening, pressing into a green body, sintering at 1100° C. to 1200° C. for 3-5 hours, and obtaining a sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass.

5. The method for preparing the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass according to claim 4, It is characterized in that In step S1, the temperature is raised from room temperature to 800°C to 900°C at a rate of 5°C / min, and after calcination, the temperature is lowered to 500°C at a rate of 5°C / min, and then cooled to room temperature in the furnace.

6. The method for preparing the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass according to claim 4, It is characterized in that The annealing temperature in step S2 is 500° C. to 600° C., and the annealing time is 5 hours.

7. The method for preparing the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass according to claim 4, It is characterized in that In the step S3, the sintering temperature is 1140° C. to 1180° C., and the holding time is 4 hours.

8. The method for preparing the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass according to claim 4, It is characterized in that In the steps S1, S2 and S3, the mass ratio of material: ball: water in ball milling is 1:2:2, and the ball milling time is 10 hours.

9. The method for preparing the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass according to claim 4, It is characterized in that The sintering system in step 3 is: heating from room temperature to 1100° C. to 1200° C. at 5° C. / min, cooling to 500° C. at 5° C. / min after sintering, and then cooling to room temperature in the furnace.

10. Use of the sodium bismuth titanate-based high-temperature energy storage ceramic material composited with glass as claimed in any one of claims 1 to 3 in a high-temperature energy storage device.

Citation Information

Patent Citations

  • High-energy-storage-density barium strontium titanate-sodium bismuth titanate-based glass ceramic composite ceramic material and preparation method thereof