Preparation of nitride combined corundum-silicon carbide composite material

Through the preparation of nitride combined with corundum-silicon carbide composite, the problem of cracking of push-plate kiln materials at high temperatures is solved, the thermal shock resistance and economic benefits are improved, and the service life of the kiln is extended.

CN118908732AActive Publication Date: 2024-11-08SINOSTEEL LUOYANG INSTITUTE OF REFRACTORIES RESEARCH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410970584.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing push-plate kiln materials are prone to cracks under high temperature load and friction resistance, and are costly, lack economic benefits and market competitiveness. Traditional refractory materials have insufficient thermal shock resistance, which affects the operating safety and service life of the kiln.

Method used

Using nitride combined with corundum-silicon carbide composite material, a specific ratio of silicon carbide, corundum, silicon powder and silica powder are mixed, and then formed in a vibration molding machine to nitride in a nitriding sintering furnace to produce nitrogen. Silicon dehydration and silicon oxynitride improve the thermal shock resistance of the material.

Benefits of technology

It improves the high-temperature flexural strength and thermal shock stability of the material, extends the service life of the kiln, reduces costs, and has broad economic and social value.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of refractory material production, in particular to preparation of a nitride combined corundum-silicon carbide composite material. The preparation method comprises the following steps: preparing 50-80wt% of silicon carbide particles, 5-20wt% of corundum particles, 5-20wt% of silicon powder, 2-12wt% of silicon dioxide micro powder, 2-5wt% of an additive and 1-2wt% of water or alcohol; wherein the corundum particles are composed of corundum particles with two different particle sizes of 0-1 mm and 1-3 mm, and the content of the corundum particles is 3-8 wt% and 5-15 wt% respectively; the silicon carbide particles are composed of three kinds of silicon carbide particles with different particle sizes of 1.5-2.5 mm, 0.5-1.5 mm and 0-0.5 mm, and the content of the silicon carbide particles is 10-15 wt%, 25-35 wt% and 10-15 wt% respectively; mixing the silicon carbide micro powder, the silicon powder and the silicon dioxide powder to obtain mixed fine powder; and loading the mixture into a mold, carrying out friction vibration molding, drying, carrying out nitridation treatment, carrying out a nitridation reaction on the green body silicon powder and the silicon dioxide micro powder to generate silicon nitride and silicon oxynitride, and cooling to room temperature along with a furnace to obtain the nitride combined corundum-silicon carbide composite material. The process is simple, the production cost is low, the product has excellent high-temperature resistance, and the thermal shock resistance is obviously superior to that of a traditional silicon nitride combined silicon carbide material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of refractory material preparation, and in particular relates to the preparation of a nitride-bonded corundum-silicon carbide composite material. Background Art

[0002] Ceramic and refractory industry pusher kiln is widely used. Usually, the performance of the pusher determines the operating efficiency of the kiln. When the pusher kiln is running, the pusher is required to withstand the load of the ceramic body or sagger, the huge top force, and the friction resistance with the track at high temperature without breaking. The service life of hot and cold cycles is as high as dozens or even hundreds of times. Therefore, the pusher is required to have excellent high temperature resistance, high mechanical strength and wear resistance, good thermal shock stability and volume stability, and no pollution to the sintering components. At the same time, the pusher and the support plate must be resistant to chemical corrosion. At present, the commonly used pushers at home and abroad are silicon carbide. The push plates made of corundum, mullite and silicon carbide are mainly made of silicon oxide combined with silicon carbide. They are prone to cracks when used in cycles. Their application range should be limited and only suitable for some low-end manufacturing fields. Traditional refractory raw materials such as corundum and mullite have many advantages, such as high load softening temperature and good creep resistance, but their strength is not ideal, the cost is high, and they lack sufficient economic benefits and market competitiveness. Push plates made of silicon nitride combined with silicon carbide have good thermodynamic properties: high high temperature strength, good thermal conductivity, small thermal expansion coefficient, acid and alkali corrosion resistance, but the thermal shock resistance needs to be further improved. Therefore, the use of advanced formulas and processes to prepare new refractory materials with high thermal shock resistance is of great significance to the service life and operation safety of push plate kilns. Summary of the invention

[0003] In order to overcome the deficiencies of the prior art, the present invention aims to provide a method for preparing a nitride-bonded corundum-silicon carbide ceramic composite material.

[0004] To achieve the above object, the technical solution adopted by the present invention is: A preparation method for a nitride-bonded corundum-silicon carbide composite material, wherein the nitride-bonded corundum-silicon carbide composite material is composed of the following raw materials in percentage by mass: 50-80wt% of silicon carbide particles, 5-20wt% of corundum particles, 5-20wt% of silicon powder, 2-12wt% of silicon dioxide micropowder, 2-5wt% of external additives, and 1-2wt% of water or alcohol; wherein the corundum particles are composed of two different particle sizes of corundum particles, 0-1mm and 1-3mm, with contents of 3-8wt% and 5-15wt% respectively; the silicon carbide particles are composed of three different particle sizes of silicon carbide particles, 1.5-2.5mm, 0.5-1.5, and 0-0.5mm, with contents of 10-15wt%, 25-35wt%, and 10-15wt% respectively; the silicon carbide micropowder, silicon powder, and silicon dioxide powder are mixed to obtain a mixed fine powder; the binder is mixed with water or alcohol; The method comprises the following steps: forming a mixed liquid; mixing silicon carbide particles and corundum particles and then uniformly mixing the mixed liquid so that the additive forms a uniform film on the surface of the particles; mixing the mixed fine powder with the mixed particles uniformly covered with the film to obtain a mixture; placing the mixture in a vibration molding machine for molding to obtain a green body; drying the obtained green body, placing it in a nitriding sintering furnace for nitriding treatment, and reacting the green body silicon powder and silicon dioxide powder together to generate silicon nitride and silicon oxynitride by nitriding reaction, and finally cooling the green body to room temperature with the furnace to prepare a nitride-bonded corundum-silicon carbide composite material.

[0005] The corundum particles are light corundum, plate corundum or a mixture of the two.

[0006] The silicon carbide powder D 50 ≤10μm, content is 5-15wt%.

[0007] The D of the silicon powder 50 ≤10μm, content is 5-20wt%.

[0008] The D of the silica powder 50 ≤10μm, content is 2-12wt%.

[0009] The additive is one or more of wood calcium, dextrin, phenolic resin and water-soluble resin, and the content is 2-5wt%.

[0010] The preparation of a nitride-bonded corundum-silicon carbide composite material proposed in the present invention has the following beneficial effects: Alumina is an oxide with excellent antioxidant properties. The thermal expansion coefficient of alumina is large, which is very different from that of silicon carbide. Introducing the corundum phase in the preparation process of silicon nitride combined with silicon carbide materials helps to preset cracks inside the material, thereby improving the thermal shock resistance of the material: Therefore, silicon carbide, corundum, silicon powder, and silicon dioxide powder are used as the main raw materials. Silicon powder and silicon dioxide powder are nitrided together to generate silicon nitride and silicon oxynitride to obtain a nitride-combined corundum-silicon carbide composite material. The production process is simple, and the product not only maintains the high-temperature flexural strength of silicon nitride combined with silicon carbide materials, but also improves the thermal shock stability of silicon nitride combined with silicon carbide, and has broad economic and social value. The volume density of the product is 2.67-2.73g / cm 3 The porosity is 14%-15%, the compressive strength at room temperature is 180-200MPa, the flexural strength at high temperature is 40-50MPa, and the thermal shock retention rate of the obtained nitride-bonded corundum-silicon carbide composite material after 5 times of water cooling at 1350℃ is ³20%, which is better than the traditional silicon nitride-bonded silicon carbide refractory material. DETAILED DESCRIPTION

[0011] The present invention will be further described below in conjunction with specific embodiments: Example 1

[0012] The mixed raw materials were weighed by mass percentage: the contents of silicon carbide particles with particle sizes of 1.5-2.5mm, 0.5-1.5, and 0-0.5mm were 15wt%, 35wt%, and 15wt%, respectively; the contents of light corundum particles with particle sizes of 0-1mm and 1-3mm were 3wt% and 5wt%, respectively; the contents of silicon carbide micropowder, silicon powder, and silicon dioxide powder were 10wt%, 12wt%, and 5wt%, respectively; and a mixed solution of wood calcium and water was added, the mass percentages of which were 2wt% and 1wt% of the total mass of the mixed raw materials, respectively. The mixed material was loaded into a mold and vibrated into shape, and after drying, it was placed in a nitriding sintering furnace and nitrided at 1420°C, and finally cooled to room temperature with the furnace to prepare a nitride-bonded corundum-silicon carbide composite material; after testing, the performance indicators of the nitride-bonded corundum-silicon carbide ceramic composite material prepared in this embodiment were: volume density 2.70g / cm 3 , porosity 15%, room temperature compressive strength 202MPa, high temperature flexural strength 46MPa, the composite material has a thermal shock retention rate of 30% after 5 times of water cooling at 1350℃. Example 2

[0013] The mixed raw materials were weighed by mass percentage: the contents of silicon carbide particles with particle sizes of 1.5-2.5mm, 0.5-1.5, and 0-0.5mm were 15wt%, 30wt%, and 15wt%, respectively; the contents of light corundum particles with particle sizes of 0-1mm and 1-3mm were 3wt% and 10wt%, respectively; the contents of silicon carbide micropowder, silicon powder, and silicon dioxide powder were 10wt%, 12wt%, and 5wt%, respectively; a mixed solution of wood calcium and water was added, and the mass percentages thereof were 2wt% and 1wt% of the total mass of the mixed raw materials, respectively; the mixed material was loaded into a mold and vibrated into shape, and after drying, it was placed in a nitriding sintering furnace and nitrided at 1420°C, and finally cooled to room temperature with the furnace to prepare a nitride-bonded corundum-silicon carbide composite material; after testing, the performance indicators of the nitride-bonded corundum-silicon carbide ceramic composite material prepared in this embodiment were: volume density 2.71g / cm 3 , porosity 14.5%, room temperature compressive strength 194MPa, high temperature flexural strength 42MPa, the composite material after 5 thermal shock retention rates of 35% at 1350℃ water cooling. Example 3

[0014] Weigh the mixed raw materials by mass percentage: the contents of silicon carbide particles with particle sizes of 1.5-2.5mm, 0.5-1.5, and 0-0.5mm are 15wt%, 30wt%, and 15wt%, respectively; the content of light corundum particles with a diameter of 1-3mm is 10wt%, the content of plate-shaped corundum particles with a diameter of 0-0.5mm is 3wt%, the contents of silicon carbide micropowder, silicon powder, and silicon dioxide powder are 10wt%, 12wt%, and 5wt%, respectively; and a mixed solution of resin and alcohol is added, the mass percentages of which are 5wt% and 1wt% of the total mass of the mixed raw materials, respectively. The mixed material is loaded into a mold and vibrated to form, and after drying, it is placed in a nitriding sintering furnace for nitriding treatment at 1420°C, and finally cooled to room temperature with the furnace to prepare a nitride-bonded corundum-silicon carbide composite material. After testing, the performance indicators of the nitride-bonded corundum-silicon carbide ceramic composite material prepared in this embodiment are: volume density 2.71g / cm 3 , porosity 14.5%, room temperature compressive strength 194MPa, high temperature flexural strength 46MPa, the composite material after 5 thermal shock retention rates of 30% at 1350℃ water cooling. Example 4

[0015] Weigh the mixed raw materials by mass percentage: the contents of silicon carbide particles with particle sizes of 1.5-2.5mm, 0.5-1.5, and 0-0.5mm are 15wt%, 30wt%, and 15wt%, respectively; the content of plate-shaped corundum particles with a diameter of 1-3mm is 10wt%, the content of light corundum particles with a diameter of 0-0.5mm is 3wt%, the contents of silicon carbide micropowder, silicon powder, and silicon dioxide powder are 10wt%, 12wt%, and 5wt%, respectively; and a mixed solution of resin and alcohol is added, the mass percentages of which are 5wt% and 1wt% of the total mass of the mixed raw materials, respectively. The mixed material is loaded into a mold and vibrated to form, and after drying, it is placed in a nitriding sintering furnace for nitriding treatment at 1420°C, and finally cooled to room temperature with the furnace to prepare a nitride-bonded corundum-silicon carbide composite material. After testing, the performance indicators of the nitride-bonded corundum-silicon carbide ceramic composite material prepared in this embodiment are: volume density 2.72g / cm 3 , porosity 14.2%, room temperature compressive strength 188MPa, high temperature flexural strength 41MPa, the composite material after 5 thermal shock retention rates of 30% at 1350℃ water cooling.

Claims

1. Preparation of a nitride-bonded corundum-silicon carbide composite material, Features: The nitride-bonded corundum-silicon carbide composite material is composed of the following raw materials in percentage by mass: 50-80wt% of silicon carbide particles, 5-20wt% of corundum particles, 5-20wt% of silicon powder, 2-12wt% of silicon dioxide micropowder, 2-5wt% of external additives, and 1-2wt% of water or alcohol; wherein the corundum particles are composed of two different particle sizes of corundum particles, 0-1mm and 1-3mm, with contents of 3-8wt% and 5-15wt% respectively; the silicon carbide particles are composed of three different particle sizes of silicon carbide particles, 1.5-2.5mm, 0.5-1.5, and 0-0.5mm, with contents of 10-15wt%, 25-35wt%, and 10-15wt% respectively; the silicon carbide micropowder, silicon powder, and silicon dioxide powder are mixed to obtain a mixed fine powder; the binder is mixed with water or alcohol; The method comprises the following steps: forming a mixed liquid; mixing silicon carbide particles and corundum particles and then uniformly mixing the mixed liquid so that the additive forms a uniform film on the surface of the particles; mixing the mixed fine powder with the mixed particles uniformly covered with the film to obtain a mixture; placing the mixture in a vibration molding machine for molding to obtain a green body; drying the obtained green body, placing it in a nitriding sintering furnace for nitriding treatment, and reacting the green body silicon powder and silicon dioxide powder together to generate silicon nitride and silicon oxynitride by nitriding reaction, and finally cooling the green body to room temperature with the furnace to prepare a nitride-bonded corundum-silicon carbide composite material.

2. Preparation of a nitride-bonded corundum-silicon carbide composite material as claimed in claim 1, Features: The corundum particles are light corundum, plate corundum or a mixture of the two.

3. Preparation of a nitride-bonded corundum-silicon carbide composite material as claimed in claim 1, Features: The silicon carbide powder D 50 ≤10μm, content is 5-15wt%.

4. The preparation of a nitride-bonded corundum-silicon carbide composite material as claimed in claim 1, Features: The D of the silicon powder 50 ≤10μm, content is 5-20wt%.

5. The preparation of a nitride-bonded corundum-silicon carbide composite material as claimed in claim 1, Features: The D of the silica powder 50 ≤10μm, content is 2-12wt%.

6. Preparation of a nitride-bonded corundum-silicon carbide composite material as claimed in claim 1, Features: The additive is one or more of wood calcium, dextrin, phenolic resin, and water-soluble resin, and the content is 2-5wt%.

Citation Information

Patent Citations

  • Phosphorous-containing nitride combined silicon carbide material and preparation method thereof

    CN108191438A

  • Solar thermal power generation and heat absorption / storage integrated corundum / SiC ceramic material and preparation method thereof