Method for preparing fine SiCN ceramic based on 3D printing and fine SiCN ceramic

By optimizing the ceramic precursor composition and process in 3D printing technology, the problems of low forming accuracy and yield in photopolymerization 3D printing technology have been solved, and high-precision and high-yield micro-SiCN ceramic preparation has been achieved, meeting the manufacturing needs of high-precision parts.

CN118908733APending Publication Date: 2024-11-08GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410843812.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing photopolymerization 3D printing technology has low forming accuracy and low ceramic yield when preparing ceramic precursors, making it difficult to meet the manufacturing needs of high-precision parts.

Method used

Micro-SiCN ceramics were prepared by 3D printing using a combination of polysilazane containing double bonds, acrylic active monomers, photoinitiators, antioxidants and light absorbers. The photosensitive properties of the ceramic precursor slurry were controlled, the printing and pyrolysis processes were optimized, and the molding accuracy and yield were improved.

Benefits of technology

High-precision forming of micro-SiCN ceramics was achieved, with a minimum feature size of 8μm, a minimum forming pore size as low as 14μm, a ceramic yield of up to 67.6%, a specific strength of up to 2.23×105N·m/kg, and excellent mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908733A_ABST
    Figure CN118908733A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ceramic materials, in particular to a method for preparing fine SiCN ceramic based on 3D printing and the fine SiCN ceramic. The preparation method adopts the following raw materials: 50-80% of polysilazane containing double bonds, 20-50% of an acrylic acid active monomer, 0.1-3% of a photoinitiator, 0.3-3% of an antioxidant and 0.01-0.5% of a light absorber. According to the method, the fine SiCN ceramic with high forming precision, high yield and good mechanical properties can be formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic materials, and in particular to a method for preparing fine SiCN ceramics based on 3D printing and the fine SiCN ceramics. Background Art

[0002] Ceramic materials have excellent properties such as high hardness, high strength, high temperature resistance, corrosion resistance, and biocompatibility, so they are widely used in aerospace, electronic information, biomedicine and other fields.

[0003] At present, additive manufacturing technology has been used to manufacture ceramic parts with complex structures. It uses silicon-based resin as a ceramic precursor and silicon-based resin precursor as raw material. Starting from the molecular structure design, it uses the polymer's easy processing to obtain a specific shape, and then converts it into ceramics through high-temperature pyrolysis. The method of additive manufacturing of ceramic precursors subverts the traditional way of preparing ceramic materials by high-temperature pyrolysis of inorganic non-metallic powders, and realizes the regulation of the microstructure and properties of ceramic materials at the atomic or molecular scale, which facilitates the integration of structure and function.

[0004] Specifically, the ceramic precursor can be printed and formed using an ordinary resin photocuring 3D printer. It uses photocuring 3D printing to prepare non-oxides from polymer-derived ceramic precursors, which has the advantages of high molding accuracy and low pyrolysis temperature. The corresponding ceramic structure can be obtained after high-temperature pyrolysis of the cured ceramic precursor green body in a vacuum or inert atmosphere. At present, polymer-derived ceramic precursors combined with photocuring 3D printing technology can be used to prepare non-oxide ceramic structures such as silicon carbide, silicon oxycarbide, silicon nitride, and silicon carbonitride. However, the molding accuracy of these technologies is still not high, and the ceramic yield is also low (usually 35% to 55%).

[0005] Nowadays, the molding accuracy of microstereolithography (PμSL) and digital light processing (DLP) 3D printing technologies can reach below 10μm, but the molding accuracy of photocuring 3D printing technology for manufacturing polymer-derived ceramic precursors is usually around 200μm, which is far from meeting the manufacturing accuracy requirements of high-precision parts.

[0006] Therefore, there is still an urgent need to explore the polymer ceramic process of photocuring 3D printing. Summary of the invention

[0007] One of the purposes of the present invention is to avoid the deficiencies in the prior art and provide a method for preparing fine SiCN ceramics based on 3D printing, which can form fine SiCN ceramics with high precision, high yield and good mechanical properties.

[0008] A second object of the present invention is to provide a fine SiCN ceramic.

[0009] To achieve one of the above purposes, the present invention provides the following technical solutions:

[0010] Provided is a method for preparing fine SiCN ceramics based on 3D printing, the raw materials used include:

[0011] Polysilazane containing double bonds 50-80%

[0012] Acrylic acid active monomer 20~50%

[0013] Photoinitiator 0.1~3%

[0014] Antioxidant 0.3~3%

[0015] Light absorber 0.01~0.5%

[0016] The preparation method comprises the following steps:

[0017] Step 1, mixing vinyl polysilazane and acrylic acid reactive monomer uniformly to obtain a premix;

[0018] Step 2: adding a photoinitiator, an antioxidant, and a light absorber to the premix, mixing them evenly to obtain a ceramic precursor slurry, using the ceramic precursor slurry as a 3D printing raw material, and obtaining a ceramic precursor body by printing;

[0019] Step three: solidifying and pyrolyzing the ceramic precursor green body in sequence to obtain ceramics.

[0020] In some embodiments, the acrylic acid reactive monomer includes one or a mixture of any two or more of 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, and polyethylene glycol diacrylate.

[0021] The double bond-containing polysilazane is vinyl polysilazane.

[0022] In some embodiments, the photoinitiator includes one or a mixture of any two or more of bis(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexylphenylacetone, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and ethyl 2,4,6-trimethylbenzoylphenylphosphonate.

[0023] In some embodiments, the antioxidant includes one of 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene (antioxidant 1330), pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate or a mixture of any two or more thereof.

[0024] In some embodiments, the light absorber includes one of Sudan I, Sudan III, Sudan Orange G, and carbon nanotubes, or a mixture of any two or more thereof.

[0025] In some embodiments, the viscosity of the ceramic precursor slurry is controlled to be 200 mPa·s to 600 mPa·s.

[0026] In some embodiments, in step three, the curing step includes: placing the ceramic precursor body in a UV curing box for curing for 1.5 to 3 hours, or placing it in a tubular furnace protected by flowing inert gas and keeping it at 180 to 250° C. for 80 to 100 minutes.

[0027] In some embodiments, in step 2, the printing parameters are: UV wavelength 405nm, light intensity 5-150mW / cm 2 , exposure time 0.5~5s, thickness of each layer 5~50μm;

[0028] In step three, the pyrolysis step includes: introducing a nitrogen atmosphere into a tubular furnace and heating the temperature from 30°C to 450°C at a heating rate of 0.5°C / min to 2°C / min, keeping the temperature for 1h to 3h, then heating the temperature to 1100°C to 1400°C at a heating rate of 0.5°C / min to 2°C / min, and keeping the temperature for 1h to 3h.

[0029] Beneficial effects of the method for preparing fine SiCN ceramics based on 3D printing of the present invention:

[0030] The method for preparing fine SiCN ceramics based on 3D printing of the present invention, wherein the photocuring 3D printing ceramic precursor slurry contains a light absorber, which can effectively reduce the photosensitivity of the entire ceramic precursor slurry, that is, when the light used for curing penetrates into the ceramic precursor slurry, the light absorber effectively absorbs the intensity of the curing light, and avoids excessive curing light from penetrating too much, causing the slurry in the remaining uncured positions in the microstructure of the cured part to be cured, so that the previously formed microstructure is cured again, affecting the accuracy of the entire microceramic structure. At the same time, when curing the current layer, the light absorber can absorb part of the scattered light, avoiding the excessive light scattering intensity affecting the curing degree of nearby materials, effectively ensuring the accuracy of photocuring, and realizing the miniaturization and precision of the microstructure.

[0031] To achieve the second objective above, the present invention provides the following technical solutions:

[0032] Provided is a fine SiCN ceramic, which is prepared by the above-mentioned method for preparing fine SiCN ceramic based on 3D printing.

[0033] In some embodiments, the minimum feature of the fine ceramic structure in the fine SiCN ceramic is 8 μm, the minimum formed pore size is as low as 14 μm, and the overall size can reach 50 mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a scanning electron microscope image of the in-plane accuracy test of the ceramic precursor body of Example 2.

[0035] Figure 2 This is a scanning electron microscope image of the minimum forming hole test of the ceramic precursor body of Example 2.

[0036] Figure 3 This is a scanning electron microscope image of the three-dimensional Gyroid lattice structure of the ceramic precursor body of Example 2.

[0037] Figure 4 This is a scanning electron microscope image of the three-dimensional Diamond lattice structure of the ceramic precursor body of Comparative Example 2.

[0038] Figure 5 This is a scanning electron microscope image of the three-dimensional Octect lattice structure of SiCN ceramics formed after pyrolysis in an inert atmosphere in Example 2.

[0039] Figure 6 This is the XRD pattern of the SiCN ceramic obtained after pyrolysis in Example 2. DETAILED DESCRIPTION

[0040] The preferred embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the preferred embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0041] The terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The singular forms of "a", "the" and "the" used in the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0042] It should be understood that although the terms "first", "second", "third", etc. may be used to describe various information in the present invention, such information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of the present invention, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0043] Example 1

[0044] The preparation method of fine SiCN ceramics based on 3D printing disclosed in this embodiment adopts raw materials including: 50-80% polysilazane containing double bonds, preferably 70%,

[0045] Acrylic acid active monomer 20-50%, preferably 30%, photoinitiator 0.1-3%, preferably 2%, antioxidant 0.3-3%, preferably 1%, light absorber 0.01-0.5%, preferably 0.1%, the preparation method comprises the following steps:

[0046] Step 1, mixing vinyl polysilazane and acrylic acid reactive monomer uniformly to obtain a premix;

[0047] Step 2: Add a photoinitiator, an antioxidant, and a light absorber to the premix, mix them evenly, and obtain a ceramic precursor slurry. After mixing evenly, perform a vacuum degassing treatment to obtain a light-cured 3D printing ceramic precursor slurry, which has low viscosity, good fluidity, stability and photosensitivity. The ceramic precursor slurry is used as a 3D printing raw material to obtain a three-dimensional structured ceramic precursor body by printing;

[0048] Step three: solidifying and pyrolyzing the ceramic precursor green body in sequence to obtain ceramics.

[0049] In this embodiment, the acrylic acid reactive monomer includes 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, polyethylene glycol diacrylate or a mixture of any two or more thereof.

[0050] The double bond-containing polysilazane is vinyl polysilazane, which is a polysilazane containing vinyl groups and has low viscosity and good reactivity. Since the side chain vinyl group has a carbon-carbon double bond, it can have a better photocuring effect and a higher crosslinking density after being photosensitively modified.

[0051] In this embodiment, the photoinitiator is a free radical photoinitiator, including one or a mixture of any two or more of bis(2,4,6-trimethylbenzoyl)phosphine oxide (photoinitiator 819), 1-hydroxycyclohexylphenylacetone (photoinitiator 184), diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (photoinitiator TPO), and ethyl 2,4,6-trimethylbenzoylphenylphosphonate (photoinitiator TPOL).

[0052] In this embodiment, the light absorber includes one of Sudan I, Sudan III, Sudan Orange G, and carbon nanotubes, or a mixture of any two or more thereof. The light absorber can change the photosensitivity of the ceramic precursor slurry and improve the printing resolution and molding accuracy.

[0053] In this embodiment, the viscosity of the ceramic precursor slurry is controlled to be 200 mpa·s to 600 mpa·s, preferably 400 mpa·s. This has a low viscosity and good fluidity, and is suitable for resin printing.

[0054] In this embodiment, in step 3, the curing step includes: placing the ceramic precursor body in a UV curing box for curing for 1.5 to 3 hours, preferably 2 hours, or placing it in a tubular furnace protected by flowing inert gas and keeping it at 180 to 250° C. for 80 to 100 minutes, preferably keeping it at 200° C. for 90 minutes;

[0055] In this embodiment, in step 2, the ceramic precursor slurry is placed in the Magic Cube microArch P150, S230 light-curing micro-nano 3D printer, and the printing parameters are: ultraviolet light wavelength 405nm, light intensity 5-150mW / cm 2 , preferably 100 mW / cm 2 The exposure time is 0.5 to 5 s, preferably 4 s, and the thickness of each layer is 5 to 50 μm, preferably 10 μm. A ceramic precursor blank with high molding accuracy and small-size molding features is obtained by photocuring printing.

[0056] In step 3, the pyrolysis step comprises: introducing a nitrogen atmosphere into a tubular furnace and heating the temperature from 30°C to 450°C at a heating rate of 0.5°C / min to 2°C / min, preferably from 30°C to 450°C at a heating rate of 1°C / min, and keeping the temperature for 1h to 3h, preferably 2h, and then heating the temperature from 1100°C to 1400°C at a heating rate of 0.5°C / min to 2°C / min, preferably from 1300°C at a heating rate of 1°C / min, and keeping the temperature for 1h to 3h, preferably 2h,

[0057] The pyrolysis process is to introduce nitrogen atmosphere into a tubular furnace and increase the temperature from 30°C to 450°C at a heating rate of 0.5-2°C / min, and keep it warm for 1-3 hours; then increase the temperature to 1100-1400°C at a heating rate of 0.5-2°C / min, and keep it warm for 1-3 hours to obtain the ceramic parts of the designed model. The ceramic shrinkage rate is 29.1%, the ceramic yield is as high as 67.6%, the hardness is as high as 13.5GPa, and the specific strength is as high as 2.23×10 5 N·m / kg; the present invention can be used to prepare micro-SiCN ceramic parts with an overall size of 50mm, a minimum characteristic size of 8μm, and a minimum forming hole diameter of 14μm. The ceramic parts obtained after the pyrolysis process have not only good forming accuracy and small-size forming characteristics, but also high ceramic yield and high mechanical properties.

[0058] In step 1, the stirring parameters of the premix are stirring speed of 600-800 r / min and stirring time of 1 h to 3 h, and the stirring parameters of the precursor slurry are stirring speed of 600-800 r / min and stirring time of 3 h to 5 h.

[0059] The present invention develops a photocurable 3D printing ceramic precursor slurry, a preparation method thereof and a ceramicization method. By adding a light absorber to improve the printing resolution, SiCN ceramics with micron-level characteristic dimensions can be prepared. Compared with the current conventional printing molding, it has high precision, small molding size characteristics, good quality, and excellent efficiency and quality.

[0060] The ceramic yield of the ceramic slurry for 3D printing of the present invention can reach more than 67.6%, which is much higher than the 20-50% ceramic yield of the prior art. The high ceramic yield means that the gas products emitted during the high-temperature pyrolysis process are small, the structure is compact, and the defects are few, which helps to improve the strength of the material and structure.

[0061] The ceramics prepared by the ceramic slurry for 3D printing of the present invention have the advantages of strong mechanical properties and a specific strength of up to 2.23×10 5 N·m / kg, higher than the existing technology.

[0062] The minimum feature of the micro-ceramic structure in the micro-SiCN ceramic is 8 μm, and the minimum forming pore size is as low as 14 μm.

[0063] The overall size can reach 50mm.

[0064] Example 2

[0065] The preparation method of fine SiCN ceramics based on 3D printing disclosed in this embodiment includes the following steps:

[0066] Weigh 75% of vinyl polysilazane and 25% of trimethylolpropane triacrylate, place the two in a magnetic stirrer and stir at a speed of 800 r / min for 2 h to mix them evenly to obtain a premix;

[0067] Add 2% bis(2,4,6-trimethylbenzoyl)phosphine oxide, 0.5% 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene and 0.2% Sudan Orange G to the above premix, place in a magnetic stirrer and stir at 800 r / min for 4 h to completely dissolve it to obtain a uniformly dispersed ceramic precursor slurry.

[0068] The uniformly mixed ceramic precursor slurry is poured into a light-curing 3D printer to print the blank. The printer parameters are set to a light intensity of 120mW / cm for the first layer. 2 , exposure time 3s, the back layer light intensity is 100mW / cm 2 , exposure time 2s, slice thickness 10μm, to obtain a first ceramic precursor green body with good molding quality, and place the first ceramic precursor green body in a 405nm UV curing box for light treatment for 6h to obtain a second ceramic precursor green body with a higher degree of cross-linking.

[0069] The second ceramic precursor blank was placed in a tube furnace, and a flowing inert atmosphere was introduced. The temperature was raised from 30°C to 450°C at a heating rate of 1°C / min and kept at that temperature for 1 hour; then the temperature was raised to 1400°C at a heating rate of 1°C / min and kept at that temperature for 2 hours to finally obtain a ceramic sintered part. The minimum molding feature size of the SiCN micro-ceramic parts was 8μm, the minimum molding hole diameter was as low as 14μm, the shrinkage rate was 29.1%, the hardness was as high as 13.5GPa, the ceramic yield was as high as 67.6%, the Diamond structure compressive strength was as high as 162.75MPa, and the corresponding specific strength was 2.23×10 5 N·m / kg.

[0070] The fine SiCN ceramics obtained in Example 2 were characterized and the following results were obtained:

[0071] Figure 1 This is a scanning electron microscope image of the in-plane accuracy test of the ceramic precursor body of Example 2. The in-plane accuracy can reach 8μm.

[0072] Figure 2 This is the scanning electron microscope image of the minimum formed pore test of the ceramic precursor body of Example 2. The diameter of the minimum formed ceramic precursor micropore is as low as 14μm.

[0073] Figure 3 This is a scanning electron microscope image of the three-dimensional Gyroid lattice structure of the ceramic precursor body of Example 2.

[0074] Figure 5 This is a scanning electron microscope image of the Octect lattice structure of SiCN ceramics formed after pyrolysis in an inert atmosphere in Example 2.

[0075] Figure 6 This is the XRD diagram of the SiCN ceramic obtained after pyrolysis in Example 2, and the interior is uncrystallized SiCN ceramic.

[0076] It can be seen that the fine SiCN ceramics prepared in this embodiment have higher precision.

[0077] Example 3

[0078] The preparation method of fine SiCN ceramics based on 3D printing disclosed in this embodiment includes the following steps:

[0079] Weigh 66.67% of vinyl polysilazane and 33.33% of trimethylolpropane triacrylate, place the two in a magnetic stirrer and stir at a speed of 800 r / min for 2 h to mix them evenly to obtain a premix;

[0080] Add 2% bis(2,4,6-trimethylbenzoyl)phosphine oxide, 0.5% 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene and 0.1% Sudan I to the above premix, place in a magnetic stirrer and stir at 800 r / min for 4 hours to completely dissolve it to obtain a uniformly dispersed ceramic precursor slurry.

[0081] The uniformly mixed ceramic precursor slurry is poured into a light-curing 3D printer to print the blank. The printer parameters are set to a light intensity of 120mW / cm for the first layer. 2 , exposure time 3s, the back layer light intensity is 100mW / cm 2 , exposure time 2s, slice thickness 10μm, to obtain a first ceramic precursor green body with good molding quality, and place the first ceramic precursor green body in a 405nm UV curing box for light treatment for 6h to obtain a second ceramic precursor green body with a higher degree of cross-linking.

[0082] The second ceramic precursor blank was placed in a tube furnace, and a flowing inert atmosphere was introduced. The temperature was raised from 30°C to 450°C at a heating rate of 1°C / min and kept at that temperature for 1 hour. The temperature was then raised to 1400°C at a heating rate of 1°C / min and kept at that temperature for 2 hours to finally obtain a ceramic sintered part. The minimum forming feature of the SiCN micro-ceramic part was 8μm, the shrinkage rate was 30.5%, the ceramic yield was 64.07%, the hardness was 11.5GPa, the Diamond structure compressive strength was 121.9MPa, and the corresponding specific strength was 1.67×10 5 N·m / kg.

[0083] Example 4

[0084] The preparation method of fine SiCN ceramics based on 3D printing disclosed in this embodiment includes the following steps:

[0085] Weigh 75% of vinyl polysilazane and 25% of trimethylolpropane triacrylate, place the three in a magnetic stirrer and stir at a speed of 800 r / min for 2 hours to mix them evenly to obtain a premix;

[0086] Add 2% bis(2,4,6-trimethylbenzoyl)phosphine oxide, 0.5% 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 0.2% Sudan Orange G, and 0.05% multi-walled carbon nanotubes to the above premix, place in a magnetic stirrer and stir at 800 r / min for 4 hours to completely dissolve it to obtain a uniformly dispersed ceramic precursor slurry.

[0087] The uniformly mixed ceramic precursor slurry is poured into a light-curing 3D printer to print the blank. The printer parameters are set to a light intensity of 100mW / cm 2 , exposure time 3s, the back layer light intensity is 50mW / cm 2 , exposure time 2s, slice thickness 10μm, to obtain a first ceramic precursor blank with good molding quality, and place the first ceramic precursor blank in a 405nm UV curing box for light treatment for 6h to obtain a second ceramic precursor blank with a higher degree of crosslinking. The second ceramic precursor blank prepared by adding carbon nanotubes has better toughness, thereby improving the printing success rate.

[0088] The second ceramic precursor green body was placed in a tube furnace, and a flowing inert atmosphere was introduced. The temperature was raised from 30°C to 450°C at a heating rate of 1°C / min and kept at that temperature for 1 hour. The temperature was then raised to 1400°C at a heating rate of 1°C / min and kept at that temperature for 2 hours to finally obtain a ceramic sintered part. The obtained ceramic part had a shrinkage rate of 29.1%, a ceramic yield of 68.1%, a hardness of up to 13.7GPa, a Diamond structure compressive strength of 110.5MPa, and a corresponding specific strength of 1.51×10 5 N·m / kg.

[0089] Example 5

[0090] The preparation method of fine SiCN ceramics based on 3D printing disclosed in this embodiment includes the following steps:

[0091] Weigh 60% of vinyl polysilazane, 20% of 1,6-hexanediol diacrylate, and 20% of trimethylolpropane triacrylate, place the three in a magnetic stirrer and stir at a speed of 800 r / min for 2 hours to mix them evenly to obtain a premix;

[0092] Add 2% bis(2,4,6-trimethylbenzoyl)phosphine oxide, 0.5% 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene and 0.1% Sudan III to the above premix, place in a magnetic stirrer and stir at 800 r / min for 4 hours to completely dissolve it to obtain a uniformly dispersed ceramic precursor slurry.

[0093] The uniformly mixed ceramic precursor slurry is poured into a light-curing 3D printer to print the blank. The printer parameters are set to a light intensity of 100mW / cm 2 , exposure time 3s, the back layer light intensity is 50mW / cm 2 , exposure time 2s, slice thickness 10μm, to obtain a first ceramic precursor green body with good molding quality, and place the first ceramic precursor green body in a 405nm UV curing box for light treatment for 6h to obtain a second ceramic precursor green body with a higher degree of cross-linking.

[0094] The second ceramic precursor green body was placed in a tube furnace, and a flowing inert atmosphere was introduced. The temperature was raised from 30°C to 450°C at a heating rate of 1°C / min and kept at that temperature for 1 hour. The temperature was then raised to 1400°C at a heating rate of 1°C / min and kept at that temperature for 2 hours to finally obtain a ceramic sintered part. The shrinkage rate of the obtained ceramic part was 31.8%, the ceramic yield was 61.2%, the Diamond structure compressive strength was 80.3MPa, and the corresponding specific strength was 1.12×10 5 N·m / kg.

[0095] Comparative Example 1

[0096] This comparative example provides a ceramic slurry for photocuring 3D printing, and its mass fraction components and preparation method are as follows:

[0097] Weigh 50% vinyl polysilazane and 50% trimethylolpropane triacrylate, place the two in a magnetic stirrer and stir at 800 r / min for 2 h to mix evenly;

[0098] Add 2% bis(2,4,6-trimethylbenzoyl)phosphine oxide, 0.5% 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene and 0.02% Sudan Orange G to the above mixed solution, place in a magnetic stirrer and stir at 800 r / min for 4 h to completely dissolve it to obtain a uniformly dispersed ceramic precursor slurry.

[0099] The uniformly mixed ceramic precursor slurry is poured into a light-curing 3D printer to print the blank. The printer parameters are set to a light intensity of 50mW / cm for the first layer. 2 , exposure time 3s, the back layer light intensity is 20mW / cm2 , exposure time 2s, slice thickness 10μm, to obtain a first ceramic precursor green body with good molding quality, and place the first ceramic precursor green body in a 405nm UV curing box for light treatment for 6h to obtain a second ceramic precursor green body with a higher degree of cross-linking.

[0100] The second ceramic precursor green body was placed in a tubular furnace, and a flowing inert atmosphere was introduced. The temperature was increased from 30°C to 450°C at a heating rate of 1°C / min and kept at that temperature for 1 hour. The temperature was then increased to 1400°C at a heating rate of 1°C / min and kept at that temperature for 2 hours. Finally, a ceramic sintered part was obtained, with a shrinkage of 34.96%, a ceramic yield of 54%, a Diamond structure compressive strength of 60.5 MPa, and a corresponding specific strength of 7.9×10 4 N·m / kg.

[0101] Comparative Example 2

[0102] This comparative example provides a ceramic slurry for photocuring 3D printing, and its mass fraction components and preparation method are as follows:

[0103] Weigh 75% of vinyl polysilazane and 25% of trimethylolpropane triacrylate, place the two in a magnetic stirrer and stir at 800 r / min for 2 h to mix them evenly;

[0104] Add 2% bis(2,4,6-trimethylbenzoyl)phosphine oxide and 0.5% 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene to the above mixed solution, place it in a magnetic stirrer and stir at 800 r / min for 4 hours to completely dissolve it to obtain a uniformly dispersed ceramic precursor slurry.

[0105] The uniformly mixed ceramic precursor slurry is poured into a light-curing 3D printer to print the blank. The printer parameters are set to a light intensity of 50mW / cm for the first layer. 2 , exposure time 3s, the back layer light intensity is 20mW / cm 2 , exposure time 2s, slice thickness 10μm, a first ceramic precursor blank with good molding quality was obtained, the first ceramic precursor blank was placed in a 405nm UV curing box for light treatment, the light treatment time was 6h, and a second ceramic precursor blank with a higher degree of crosslinking was obtained. The ceramic precursor blank prepared without adding a light absorber has poor in-plane molding accuracy, with a minimum molding feature of 60μm, a minimum molding depth of 2mm, and a hole diameter greater than 500μm.

[0106] Figure 4 This is a scanning electron microscope image of the three-dimensional Diamond lattice structure of the ceramic precursor blank of Comparative Example 2. It can be seen from the image that the molding accuracy is poor.

[0107] Comparative Example 3

[0108] This comparative example provides a ceramic slurry for photocuring 3D printing, and its mass fraction components and preparation method are as follows:

[0109] Weigh 75% polysilazane and 25% trimethylolpropane triacrylate, place the two in a magnetic stirrer and stir at 800 r / min for 2 h to mix them evenly;

[0110] Add 2% bis(2,4,6-trimethylbenzoyl)phosphine oxide and 0.5% 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene to the above mixed solution, place it in a magnetic stirrer and stir at 800 r / min for 4 hours to completely dissolve it to obtain a uniformly dispersed ceramic precursor slurry.

[0111] The uniformly mixed ceramic precursor slurry is poured into a light-curing 3D printer to print the blank. The printer parameters are set to a light intensity of 50mW / cm for the first layer. 2 , exposure time 3s, the back layer light intensity is 20mW / cm 2 , exposure time 2s, slice thickness 10μm, and the first ceramic precursor blank with good molding quality was obtained. Polysilazane is difficult to print completely due to its lack of vinyl, low reaction activity, and poor photo-crosslinking curing effect.

[0112] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing fine SiCN ceramics based on 3D printing, It is characterized in that The raw materials used include: Polysilazane containing double bonds 50% to 80% Acrylic acid active monomer 20%~50% Photoinitiator 0.1%~3% Antioxidants 0.3% to 3% Light absorber 0.01%~0.5% The preparation method comprises the following steps: Step 1, mixing vinyl polysilazane and acrylic acid reactive monomer uniformly to obtain a premix; Step 2: adding a photoinitiator, an antioxidant, and a light absorber to the premix, mixing them evenly to obtain a ceramic precursor slurry, using the ceramic precursor slurry as a 3D printing raw material, and obtaining a ceramic precursor body by printing; Step three: solidifying and pyrolyzing the ceramic precursor green body in sequence to obtain ceramics.

2. The method for preparing fine SiCN ceramics based on 3D printing according to claim 1, It is characterized in that The acrylic acid active monomer includes one of 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, polyethylene glycol diacrylate or a mixture of any two or more thereof. The double bond-containing polysilazane is vinyl polysilazane.

3. The method for preparing fine SiCN ceramics based on 3D printing according to claim 1, It is characterized in that The photoinitiator includes one of bis(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexyl phenylacetone, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and ethyl 2,4,6-trimethylbenzoylphenylphosphonate, or a mixture of any two or more thereof.

4. The method for preparing fine SiCN ceramics based on 3D printing according to claim 1, It is characterized in that The antioxidant includes one of 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and octadecylβ-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate or a mixture of any two or more thereof.

5. The method for preparing fine SiCN ceramics based on 3D printing according to claim 1, It is characterized in that The light absorber includes one of Sudan I, Sudan III, Sudan Orange G, and carbon nanotubes, or a mixture of any two or more thereof.

6. The method for preparing fine SiCN ceramics based on 3D printing according to claim 1, It is characterized in that The viscosity of the ceramic precursor slurry is controlled to be 200 mpa·s to 600 mpa·s.

7. The method for preparing fine SiCN ceramics based on 3D printing according to claim 1, It is characterized in that In step three, the curing step includes: placing the ceramic precursor body in a UV curing box for curing for 1.5 hours to 3 hours, or placing it in a tubular furnace protected by flowing inert gas and keeping it at 180° C. to 250° C. for 80 minutes to 100 minutes.

8. The method for preparing fine SiCN ceramics based on 3D printing according to claim 1, It is characterized in that In step 2, the printing parameters are: UV wavelength 405nm, light intensity 5mW / cm 2 ~150mW / cm 2 , exposure time 0.5s~5s, thickness of each layer 5μm~50μm; In step three, the pyrolysis step includes: introducing a nitrogen atmosphere into a tubular furnace and heating the temperature from 30°C to 450°C at a heating rate of 0.5°C / min to 2°C / min, keeping the temperature for 1h to 3h, then heating the temperature to 1100°C to 1400°C at a heating rate of 0.5°C / min to 2°C / min, and keeping the temperature for 1h to 3h.

9. A fine SiCN ceramic, It is characterized in that The ceramic is prepared by the method for preparing fine SiCN ceramics based on 3D printing as described in any one of claims 1 to 9.

10. The fine SiCN ceramic according to claim 9, It is characterized in that The minimum feature of the fine ceramic structure in the fine SiCN ceramic reaches 8 μm, the minimum forming pore diameter is as low as 14 μm, and the overall size can reach 50 mm.