Porous ceramic prepared from marine waste shells and preparation method of porous ceramic

By optimizing the ratio of shells and diatomaceous earth and the sintering process, porous ceramics with high water absorption and porosity are prepared, which solves the problems of degraded performance and high cost of existing ceramics, and realizes environmentally friendly and economical ceramic preparation.

CN118908746APending Publication Date: 2024-11-08WUHAN UNIV OF TECH

Patent Information

Application Number
CN202411012895.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing porous ceramics prepared with shells as raw materials have problems such as low water absorption and porosity, reduced performance during recycling, and high production costs.

Method used

Porous ceramics are prepared using a ratio of 100 parts of shell mixture and 10 to 50 parts of pore-forming agent. The shell mixture includes 50 to 80 wt% diatomaceous earth and 20 to 50 wt% shell raw materials, and are made of ball milling, sieved, ball-forming, and aging. , drying and sintering treatment, sintering temperature is 1020-1260℃, heating rate is 3-5℃/min, sintering insulation time is 0.5-3.5h, graphite, gluten or corn starch is used as pore-making agents.

Benefits of technology

It reduces production costs by 20 to 40%, improves the water absorption, porosity and mechanical properties of porous ceramics, has good recycling performance, and is in line with the concept of sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908746A_ABST
    Figure CN118908746A_ABST
Patent Text Reader

Abstract

The invention provides porous ceramic prepared from marine waste shells and a preparation method of the porous ceramic. The porous ceramic is prepared from the following raw materials in parts by mass: 100 parts of a shell-containing mixture and 10-50 parts of a pore forming agent, wherein the shell-containing mixture comprises the following components in percentage by mass: 50-80 wt% of diatomite and 20-50 wt% of a shell raw material; according to the invention, the porous ceramic is prepared from the marine waste shells, the raw material diatomite is a green mineral resource with low price, the shells are stacked marine solid wastes, and the prepared porous ceramic can be repeatedly used, so that the production cost is reduced by 20-40%, and the porous ceramic has environmental protection significance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic materials, and in particular to a porous ceramic prepared from marine waste shells and a preparation method thereof. Background Art

[0002] Due to its unique porous structure, porous ceramics are often regarded as important carriers in the fields of catalysis and adsorption. Shells are a kind of solid waste generated in fishery production and daily life, and the accumulation is very large, especially in coastal areas. The large amount of accumulated shells not only occupies land resources, but also causes serious pollution to natural resources such as water and air. The main inorganic component of shells is CaCO3, which will decompose into CaO and CO2 at high temperature. Among them, CaO is easy to participate in the reaction to form diopside during the sintering process of silicon-calcium system ceramics, which improves the strength of ceramics; CO2 is a gas that escapes from the green body during the firing process of ceramics, increasing the porosity of ceramics. Therefore, shells can be used as an excellent raw material for preparing ceramics. However, porous ceramics prepared with shells as raw materials still have problems such as low water absorption and porosity, decreased performance during recycling, and high production costs.

[0003] Therefore, there is an urgent need for a porous ceramic prepared from marine waste shells and a preparation method thereof to solve the above-mentioned technical problems. Summary of the invention

[0004] The purpose of the present invention is to solve the technical problem of high production cost of porous ceramics prepared with shells as raw materials.

[0005] In order to solve the above technical problems, the present invention first provides a porous ceramic prepared by using marine waste shells, wherein the porous ceramic is prepared from the following raw materials in parts by weight: 100 parts of a shell-containing mixture, 10 to 50 parts of a pore-forming agent; The shell-containing mixture includes, by mass percentage, 50-80 wt% diatomaceous earth and 20-50 wt% shell raw material. Preferably, the composition of diatomaceous earth includes, by mass percentage, 80-90 wt% SiO2, 5-6 wt% Al2O3, and 1-2 wt% Fe2O3.

[0006] Preferably, the composition of the shell raw material includes, by mass percentage: 50-60wt% CaO, 40-50wt% loss on ignition.

[0007] Preferably, the shell-containing mixture further comprises greater than 0 and less than 30 wt% of magnesite in terms of mass percentage.

[0008] Preferably, the composition of the magnesite includes, by mass percentage, 30-50wt% MgO, 5-25wt% SiO2, and 30-50wt% loss on ignition.

[0009] Preferably, the pore former is at least one of graphite, gluten and corn starch.

[0010] Accordingly, the present invention further provides a method for preparing a porous ceramic prepared from marine waste shells as described in any one of the above items, comprising: S10, ball-milling the shell-containing mixture and sieving it for later use; S20, mixing the shell mixture, the pore-forming agent and water to form a spherical green body; S30, sealing the spherical green body and performing an aging treatment; S40, drying the spherical green body and sintering it to obtain a porous ceramic.

[0011] Preferably, step S20 specifically includes: S21, mixing the shell-containing mixture with a pore-forming agent to obtain a first mixture; S22, mixing the first mixed material with water to obtain a second mixed material; S23, using a spheronizer to form the second mixed material into spherical green bodies.

[0012] Preferably, in step S22, the mass of water added is 60-70wt% of the first mixture; in step S23, the diameter of the spherical green body is 8-12mm.

[0013] Preferably, in step S40, the temperature for drying the spherical green body is 70-85°C; in the sintering process, the sintering atmosphere is oxygen, the sintering temperature is 1020-1260°C, the heating rate is 3-5°C / min, and the sintering holding time is 0.5-3.5h.

[0014] The beneficial effects of the present invention are as follows: Different from the prior art, the present invention provides a porous ceramic prepared by utilizing marine waste shells and a preparation method thereof, wherein the porous ceramic is prepared from the following raw materials in proportion by mass: 100 parts of a shell-containing mixture and 10 to 50 parts of a pore-forming agent; wherein the shell-containing mixture comprises, by mass percentage, 50 to 80 wt% diatomaceous earth and 20 to 50 wt% shell raw material; the present invention prepares porous ceramics by utilizing marine waste shells, the raw material diatomaceous earth used is a low-cost green mineral resource, and the shells are accumulated marine solid waste, and the prepared porous ceramics can be reused, thereby reducing the production cost by 20 to 40%, and having environmental protection significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 A flow chart of a method for preparing porous ceramics using marine waste shells provided in an embodiment of the present invention; Figure 2A photo of a finished product of a porous ceramic material prepared from marine waste shells provided in Example 1 of the present invention; Figure 3 This is a SEM image of a porous ceramic material prepared from marine waste shells provided in Example 1 of the present invention; Figure 4 This is the XRD diagram of the porous ceramic material prepared using marine waste shells provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] In view of the problems of the prior art, the present invention prepares porous ceramics through marine waste shells. The raw material diatomaceous earth used is a low-cost green mineral resource, and the shells are accumulated marine solid waste. The prepared porous ceramics can be reused, which reduces the production cost by 20-40% and has environmental protection significance.

[0018] The present invention first provides a porous ceramic prepared by using marine waste shells. The porous ceramic is prepared from the following raw materials in parts by weight: 100 parts of a shell-containing mixture, 10 to 50 parts of a pore-forming agent; Among them, the shell-containing mixture includes, by mass percentage: 50-80wt% diatomaceous earth and 20-50wt% shell raw material.

[0019] In the embodiment of the present invention, the composition of diatomaceous earth includes, by mass percentage: 80-90wt% SiO2, 5-6wt% Al2O3, and 1-2wt% Fe2O3.

[0020] Specifically, diatomaceous earth is also a relatively abundant and economical material. When used in combination with shell raw materials, it further controls the cost of raw materials while ensuring product performance.

[0021] In an embodiment of the present invention, the components of the shell raw material include, by mass percentage: 50-60wt% CaO, 40-50wt% loss on ignition, and the content of other impurities does not exceed 1wt%.

[0022] Specifically, shells, as marine waste, are widely available and low-cost. Using a large amount of shells as raw materials not only reduces the procurement cost of raw materials, but also effectively solves the environmental pollution and resource waste problems caused by the large accumulation of shells.

[0023] In an embodiment of the present invention, the shell-containing mixture also includes greater than 0 and less than 30wt% of dolomite in terms of mass percentage.

[0024] Specifically, the composition of magnesite includes, by mass percentage: 30-50wt% MgO, 5-25wt% SiO2, 30-50wt% loss on ignition, and the content of other impurities does not exceed 1wt%.

[0025] Specifically, the combination of 50~80wt% diatomaceous earth and 20~50wt% shell raw materials, during the subsequent firing process, substances such as calcium oxide in the shell may react with components such as silicon dioxide in the diatomaceous earth to form new phases, which will help improve the strength and stability of the porous ceramics; at the same time, the appropriate addition of 0~30wt% dolomite may also form phases such as magnesium-aluminum spinel with reinforcing effects at high temperatures, further improving the mechanical properties and thermal stability of the porous ceramics.

[0026] In an embodiment of the present invention, the pore former is at least one of graphite, gluten and corn starch.

[0027] Specifically, when 10-50wt% of pore formers are added, abundant pores can be formed, making the ceramic have a high porosity. This porous structure is conducive to the permeation, adsorption and storage of gases and liquids, and can be used in the fields of filtration, adsorption, catalyst carriers, etc.

[0028] The present invention uses marine waste shells and natural mineral diatomaceous earth as main raw materials to prepare porous ceramics, thereby reducing the demand for mining traditional ceramic raw materials (such as clay, feldspar, etc.), reducing the consumption of natural resources, and complying with the concept of sustainable development.

[0029] Accordingly, see Figure 1 The present invention further provides a method for preparing a porous ceramic using marine waste shells as described above, the method comprising: S10, ball-milling the shell-containing mixture and sieving it for later use; Specifically, step S10 also includes: First, a shell-containing mixture is provided, which includes, by mass percentage, 50-80wt% diatomaceous earth and 20-50wt% shell raw material.

[0030] In an embodiment of the present invention, the shell-containing mixture also includes greater than 0 and less than 30wt% of magnesite in terms of mass percentage; wherein the components of the magnesite include, in terms of mass percentage: 30-50wt% MgO, 5-25wt% SiO2, and 30-50wt% loss on ignition.

[0031] Afterwards, the shell-containing mixture was ball-milled using a ball mill, and the ball-milled diatomaceous earth and shell raw materials were sieved through a 250-mesh sieve (61 μm) respectively.

[0032] Specifically, the purpose of passing the ball-milled shell-containing mixture through a 250-mesh sieve is mainly to: control particle size distribution: passing through a 250-mesh sieve can make the particle size of the shell-containing mixture more uniform. Uniform particle size helps the raw materials to react and combine more fully and evenly during the subsequent batching, mixing and firing processes, thereby ensuring the consistency and stability of the performance of the porous ceramic product.

[0033] S20, mixing the shell-containing mixture, the pore-forming agent and water to form a spherical green body.

[0034] Specifically, step S20 also includes: S21, mixing the shell-containing mixture with a pore-forming agent to obtain a first mixture; this allows the two raw materials to fully contact and mix, laying the foundation for the subsequent formation of a uniform porous ceramic material.

[0035] S22, mixing the first mixture with water to obtain a second mixture; wherein a proper amount of water helps the first mixture to form a slurry with certain fluidity and plasticity, which is convenient for subsequent ball-forming operations.

[0036] S23, using a spheronizer to form the second mixed material into a spherical green body; wherein, forming the second mixed material into a spherical green body is conducive to maintaining a relatively uniform shape and size during the subsequent sintering process, thereby obtaining a porous ceramic product with relatively consistent performance.

[0037] Preferably, in step S22, the mass of water added is 60-70wt% of the first mixture; the specific water-to-material ratio can ensure that the moisture of the mixture is moderate, neither too dry to make it difficult to shape, nor too moist to affect the structural stability of the green body.

[0038] Preferably, in step S23, the diameter of the spherical green body is 8-12 mm. Controlling the diameter of the spherical green body within the range of 8-12 mm not only facilitates molding and processing, but also helps to evenly transfer heat during sintering, thereby ensuring the uniformity of the internal structure of the ceramic.

[0039] S30, sealing the spherical green body and performing an aging treatment.

[0040] Specifically, step S30 also includes: The spherical green body obtained by balling is sealed and aged at room temperature until the moisture distribution is uniform; wherein, during the balling process, although water is mixed with the second mixture, there may be uneven moisture distribution; through aging, in a sealed environment, the moisture can gradually be evenly distributed inside the green body by molecular diffusion, so that the moisture content of each part tends to be consistent.

[0041] S40, drying the spherical green body and sintering it to obtain a porous ceramic.

[0042] Specifically, step S40 also includes: First, the spherical green body is dried at a drying temperature of 70-85°C. The drying temperature of 70-85°C is relatively mild and will not cause the water inside the spherical green body to evaporate too quickly and generate excessive internal stress, thereby being able to better maintain the shape and structural integrity of the spherical green body.

[0043] Secondly, the spherical green body is sintered to obtain porous ceramics; the sintering method is pressureless solid phase sintering, the sintering atmosphere is oxygen, the sintering temperature is 1020~1260℃, the sintering heating rate is 3~5℃ / min, and the sintering holding time is 0.5~3.5h.

[0044] Specifically, pressureless solid phase sintering is a relatively simple and low-cost sintering method. It does not require complex pressurizing equipment and molds, reducing the investment in production equipment and production costs. It can make the raw material particles combine with each other in the solid state through diffusion, mass transfer and other processes to form a ceramic material with certain strength and performance.

[0045] Specifically, the sintering atmosphere of oxygen helps promote the oxidative decomposition and combustion of organic matter, removes residual organic matter in the spherical green body, reduces pores and defects caused by volatilization or decomposition of organic matter during the sintering process, and improves the quality of porous ceramics.

[0046] Specifically, when the sintering temperature is 1020~1260℃, different raw materials can form the desired phase and microstructure, thereby giving the porous ceramics the desired properties, such as porosity, strength, thermal stability, etc.

[0047] Specifically, a moderate heating rate can control the temperature gradient inside the green body, reduce the thermal stress caused by excessive temperature difference, and reduce the risk of green body cracking. A suitable heating rate can also give the raw material particles enough time to diffuse and react, making the microstructure of the porous ceramic more uniform and dense.

[0048] Specifically, the heat preservation process can make the physical and chemical reactions inside the ceramic more fully proceed, so that the processes such as crystal growth, pore discharge, and phase transformation can reach a more ideal state. By controlling the heat preservation time, the porosity, strength, and microstructure of the porous ceramic can be adjusted to meet the requirements of porous ceramic performance in different application scenarios.

[0049] In order to further understand the present invention, the preparation method of the porous ceramics prepared by using marine waste shells provided by the present invention is described below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0050] Embodiment 1: Embodiment 1 of the present invention provides a method for preparing porous ceramics using marine waste shells, and the preparation method specifically comprises: Step 1, ball milling and screening: Use a ball mill to ball mill the shell mixture, and pass the ball-milled diatomaceous earth and shell raw materials through a 250-mesh sieve respectively.

[0051] Step 2: Mixing ingredients: weigh and mix the shell-containing mixture and the pore-forming agent according to their mass percentages to obtain a mixture; wherein the shell-containing mixture includes, by mass percentage: 60wt% diatomaceous earth, 30wt% shell raw material, and 10wt% magnesite; the pore-forming agent is corn starch, and the amount added is 20wt% of the shell-containing mixture.

[0052] Step 3, balling: adding water as a binder, and using a balling machine to make the mixture into spherical green bodies; wherein the mass of the added water is 65wt% of the mixture, and the diameter of the obtained spherical green bodies is 10mm.

[0053] Step 4, aging: sealing the spherical green body obtained by balling, and aging at 25° C. until the moisture distribution is uniform; Step 5, drying and firing: drying the spherical green body at 80°C, and firing at 1100°C to obtain porous ceramics; wherein the sintering method is pressureless solid phase sintering, the sintering atmosphere is oxygen, the firing heating rate is 5°C / min, and the firing holding time is 1h.

[0054] After testing, the porous ceramic provided in Example 1 of the present invention has a water absorption rate of 103.18%, a porosity of 70.58%, a compressive strength of up to 1.36 MPa, and a bulk density of 0.68 g / cm 3 After 10 cycles of water absorption, the ceramic water absorption rate still remains above 98%, and the repeated water absorption rate (10 times) ≥95%, exceeding the repeated water absorption rate (5 times) ≥70% specified in the industry standard (NY / T886-2022 Agricultural and Forestry Water Retention Agent).

[0055] See also Figures 2 to 3 , Figure 2A photo of a finished product of a porous ceramic material prepared from marine waste shells provided in Example 1 of the present invention; Figure 3 The SEM image (scanning electron microscope image) of the porous ceramic material prepared from marine waste shells provided in Example 1 of the present invention; wherein Figure 3 It can be seen that the porous ceramic material prepared from marine waste shells provided in Example 1 of the present invention has a large porosity and a uniform distribution of pore sizes, which meets the expected design requirements.

[0056] See also Figure 4 , Figure 4 The XRD diagram (X-ray diffraction diagram) of the porous ceramic material prepared from marine waste shells provided in Example 1 of the present invention; wherein Figure 4 It can be seen that the porous ceramic materials have Quartz.syn (SiO2) quartz crystal structure, Cristobalite (SiO2) cristobalite crystal structure and Wollastonite 1A (CaSiO3) wollastonite crystal structure respectively.

[0057] Specifically, the Quartz.syn (SiO2) quartz crystal structure has one diffraction peak, which appears at around 26°; the Cristobalite (SiO2) cristobalite crystal structure has three diffraction peaks, which appear at 21°, 31° and 36° respectively, and the strongest diffraction peak appears at around 21°; the Wollastonite 1A (CaSiO3) wollastonite crystal structure has three diffraction peaks, which appear at 25° to 30°, and the strongest diffraction peak appears at around 30°.

[0058] Compared with the prior art, the porous ceramics prepared from marine waste shells in the present invention have excellent performance, with a water absorption rate of 103.18%, a porosity of 70.58%, and a compressive strength of 1.36 MPa. After 10 cycles of water absorption, the water absorption rate of the ceramics is still maintained above 98%, and the repeated water absorption rate (10 times) is ≥95%. It has good recycling performance and can be used as a matrix of water-retaining and fertilizer-retaining materials and applied in the field of agricultural production.

[0059] The present invention utilizes marine waste shells to prepare porous ceramics. The raw material diatomaceous earth used is a low-cost green mineral resource, and the shells are accumulated marine solid waste. The production process adopts conventional pressureless oxidation atmosphere sintering. The prepared porous ceramics can be used repeatedly, which reduces the production cost by 20-40% and has environmental protection significance.

[0060] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.

[0061] The above embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A porous ceramic made from marine waste shells, It is characterized in that The porous ceramic is prepared from the following raw materials in parts by mass: 100 parts of a shell-containing mixture and 10 to 50 parts of a pore-forming agent; Wherein, the shell-containing mixture includes, by mass percentage: 50-80wt% diatomaceous earth and 20-50wt% shell raw material.

2. The porous ceramics prepared from marine waste shells according to claim 1, It is characterized in that The composition of the diatomaceous earth includes, by mass percentage: 80-90wt% SiO 2 、5~6wt%Al 2 O 3 、1~2wt%Fe 2 O 3 .

3. The porous ceramics prepared from marine waste shells according to claim 1, It is characterized in that The components of the shell raw material include, by mass percentage: 50-60wt% CaO, 40-50wt% loss on ignition.

4. The porous ceramics prepared from marine waste shells according to claim 1, It is characterized in that The shell-containing mixture also includes greater than 0 and less than 30wt% of dolomite in terms of mass percentage.

5. The porous ceramics prepared from marine waste shells according to claim 4, It is characterized in that The composition of the magnesite includes, by weight percentage: 30-50 wt% MgO, 5-25 wt% SiO 2 , 30~50wt% loss on ignition.

6. The porous ceramics prepared from marine waste shells according to claim 1, It is characterized in that The pore-forming agent is at least one of graphite, gluten and corn starch.

7. A method for preparing a porous ceramic prepared from marine waste shells as claimed in any one of claims 1 to 6, It is characterized in that include: S10, ball-milling the shell-containing mixture and sieving it for later use; S20, mixing the shell-containing mixture, the pore-forming agent and water to form a spherical green body; S30, sealing the spherical green body and performing an aging treatment; S40, drying the spherical green body and sintering it to obtain the porous ceramic.

8. The method for preparing porous ceramics using marine waste shells according to claim 7, It is characterized in that The step S20 specifically includes: S21, mixing the shell-containing mixture with the pore-forming agent to obtain a first mixture; S22, mixing the first mixed material with water to obtain a second mixed material; S23, using a spheronizer to form the second mixed material into the spherical green body.

9. The method for preparing porous ceramics using marine waste shells according to claim 8, It is characterized in that In the step S22, the mass of the added water is 60-70wt% of the first mixture; in the step S23, the diameter of the spherical green body is 8-12mm.

10. The method for preparing porous ceramics using marine waste shells according to claim 7, It is characterized in that In the step S40, the temperature for drying the spherical green body is 70-85°C; in the sintering process, the sintering atmosphere is oxygen, the sintering temperature is 1020-1260°C, the heating rate is 3-5°C / min, and the sintering holding time is 0.5-3.5h.

Citation Information

Patent Citations

  • Diatomaceous micropore ceramic filter cartridge and preparation method thereof

    CN101397215A

  • Ceramic material with multi-stage duct structure and manufacture method thereof

    CN101885620A

  • Preparation method of diatomite-based porous ceramic microspheres

    CN102391011A

  • Thermal insulation ceramic tile and preparation method thereof

    CN115536425A

Cited By

  • Porous ceramic modified water and fertilizer retention material as well as preparation method and application thereof

    CN119591443A

  • Method for preparing silicon carbide membrane support from shellfish shell residues

    CN120838193A