Silicon carbon material containing SiNx / Si composite silicon layer and preparation method thereof
By depositing a SiNx/Si composite silicon layer on a carbon substrate, the problem of decreased cycle performance caused by volume expansion during lithiation of silicon-carbon materials is solved, achieving efficient lithium-ion migration and stable battery performance, making it suitable for lithium-ion battery anode materials.
Patent Information
- Application Number
- CN202411030235.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-08
AI Technical Summary
Existing silicon-carbon materials suffer from significant volume expansion differences during lithiation, leading to separation of the silicon layer from the carbon substrate and a rapid decrease in cycle performance, failing to meet the requirements for high energy density and stability.
By depositing a SiNx/Si composite silicon layer on a carbon substrate, the volume expansion is mitigated by the Si3N4 ceramic phase, and the non-stoichiometric SiNx promotes the formation of the SEI film. It combines nitrogen-containing free radicals with silicon free radicals to form a nano-intercalation structure, uniformly disperses nano-silicon particles, and prevents electrochemical sintering.
It improves lithium-ion migration rate and material cycle performance, maintains high battery capacity and first coulombic efficiency, has good cycle stability, and has a simple and low-cost process.
Smart Images

Figure CN118908750A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of chemical processes, and in particular to a silicon-carbon material containing a SiNx / Si composite silicon layer and a preparation method thereof. Background Art
[0002] The rapid development of new energy technologies has led to an urgent need for high-performance electrode materials. The theoretical capacity of the currently used graphite negative electrode material is only 372mAh / g. In order to meet the requirements of high energy density, silicon materials have become an ideal choice of negative electrode materials due to their excellent lithium storage performance. Its lithium storage capacity at room temperature is as high as 3579mAh / g, which is nearly 10 times that of graphite materials. During the process of lithium ion insertion and extraction, the structure of silicon materials shows good stability. In addition, the lithium insertion potential of silicon materials is slightly higher than that of graphite, which helps to reduce the risk of lithium dendrite formation. Silicon materials are not only abundant in resources and low in cost, but also environmentally friendly and have great commercial prospects.
[0003] The chemical vapor deposition (CVD) method has uniform deposition and good winding properties, and is one of the commonly used negative electrode preparation technologies. The silicon-carbon material obtained by depositing silicon on a carbon substrate has chemical bonding at the silicon-carbon interface, which can effectively alleviate volume expansion. This method is simple in process, conducive to industrial production, and has been widely used. However, the volume expansion of the above-mentioned carbon and silicon materials during the complete lithiation process is very different (10% and 300% respectively). Excessive silicon content will cause the silicon layer to separate from the carbon substrate, resulting in a rapid decrease in cycle performance. Summary of the invention
[0004] To achieve the above-mentioned purpose of the invention, the technical solution of the present invention is as follows:
[0005] A method for preparing a silicon-carbon material containing a SiNx / Si composite silicon layer comprises placing a carbon substrate in a tubular furnace, introducing a silicon source and a nitrogen source simultaneously in a certain ratio at a certain temperature and reaching a certain gas pressure, and obtaining a SiNx composite silicon layer by a vapor deposition method.
[0006] As a preferred embodiment, the silicon layer contains Si 3 N 4 Ceramic phase and non-stoichiometric SiNx, Si 3 N 4The ceramic phase is not electrochemically active, and as an inert phase it alleviates the volume expansion of silicon materials during lithium embedding. The non-stoichiometric SiNx has a certain electrochemical activity, providing a certain capacity while promoting the formation of a nitrogen-containing SEI film, thereby increasing the lithium ion migration rate of the electrode. At the same time, during vapor deposition, the combination of nitrogen-containing radicals and silicon-containing radicals has a certain competitive effect with the bonding between silicon and silicon, reducing the particle size of silicon particles and obtaining a SiNx / Si nano-intercalated structure. SiNx not only evenly disperses the nano-silicon particles, but also prevents electrochemical sintering during the material cycle, thereby improving the material's cycle performance.
[0007] As a preferred embodiment, the carbon substrate has electrical conductivity and a certain lithium storage capacity, and is selected from graphite, hard carbon, porous carbon, or carbon nanotube materials.
[0008] As a preferred embodiment, the vapor deposition is chemical vapor deposition (CVD) or plasma enhanced chemical vapor deposition (PECVD), with a temperature range of 300° C.-800° C. and a power of 100-500W.
[0009] As a preferred embodiment, the silicon source is silane, and the nitrogen source is one or more of ammonia, nitrogen, and nitrogen trifluoride.
[0010] As a preferred embodiment, the volume ratio of the silicon source to the nitrogen source is between 5 and 0.2.
[0011] As a preferred embodiment, if the deposition method is chemical vapor deposition (CVD), the gas pressure range is 100-3000 Pa, and the temperature range is 400° C.-600° C.
[0012] As a preferred embodiment, if the deposition method is plasma enhanced chemical vapor deposition (PECVD), the gas pressure range is 0-100 Pa, the temperature range is 300° C.-600° C., and the power is 100-500W.
[0013] As a preferred method, the carbon substrate is placed in a tubular furnace, argon gas is introduced, the temperature is raised to 300-800°C at 5°C / min, and then a silicon source and a nitrogen source are introduced simultaneously in a certain proportion and a certain gas pressure is reached, and a SiNx composite silicon layer is obtained by vapor deposition.
[0014] The second object of the present invention is to provide a composite silicon layer containing SiNx / Si obtained by the preparation method, the internal structure of which is an inter-embedded structure of nano-SiNx and nano-silicon, wherein the nano-silicon particles are smaller than 5nm.
[0015] The beneficial effects of the present invention are:
[0016] Compared with ordinary CVD silicon-carbon composite materials, the silicon-carbon material containing the SiNx / Si composite silicon layer in the present invention has the following advantages: 1. The SiNx / Si composite silicon layer promotes the formation of a nitrogen-containing SEI film, thereby increasing the lithium ion migration rate of the electrode. 2. The construction of the SiNx / Si nano-inter-embedded structure evenly disperses the nano-silicon particles, while preventing electrochemical sintering during the material cycle process, thereby improving the material's cycle performance. 3. The process is simple, matching the most common CVD silicon-carbon material preparation process, without the need to introduce new processes and equipment, and has a low application cost.
[0017] The silicon-carbon composite material in the present invention has a high first coulombic efficiency when used as a negative electrode material for a lithium ion battery, and has a large battery capacity and good cycle stability. It is a lithium ion battery negative electrode material with great application potential. The prepared lithium ion battery has a first coulombic efficiency of 78-85% and a first-week discharge capacity of 1500-2600mAh / g under the test condition of a first-cycle current of 200mA / g, and has a high cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of the silicon-carbon material structure of the composite silicon layer containing SiNx / Si of the present invention.
[0019] Figure 2 It is the 0.5C long cycle diagram of the materials in Example 3 and Comparative Example 1.
[0020] Figure 3 This is the XRD diagram of Example 2 after being heated at 800°C for 1 hour under argon protection. DETAILED DESCRIPTION
[0021] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0022] The embodiment provides a method for preparing a silicon-carbon material containing a SiNx / Si composite silicon layer, wherein a carbon substrate is placed in a tubular furnace, a silicon source and a nitrogen source are introduced simultaneously in a certain ratio at a certain temperature and a certain gas pressure is reached, and a SiNx composite silicon layer is obtained by a vapor deposition method.
[0023] The silicon layer contains Si 3 N 4 Ceramic phase and non-stoichiometric SiNx, Si 3 N 4The ceramic phase is not electrochemically active, and as an inert phase it alleviates the volume expansion of silicon materials during lithium embedding. The non-stoichiometric SiNx has a certain electrochemical activity, providing a certain capacity while promoting the formation of a nitrogen-containing SEI film, thereby increasing the lithium ion migration rate of the electrode. At the same time, during vapor deposition, the combination of nitrogen-containing radicals and silicon-containing radicals has a certain competitive effect with the bonding between silicon and silicon, reducing the particle size of silicon particles and obtaining a SiNx / Si nano-intercalated structure. SiNx not only evenly disperses the nano-silicon particles, but also prevents electrochemical sintering during the material cycle, thereby improving the material's cycle performance.
[0024] In some embodiments, the carbon substrate has electrical conductivity and a certain lithium storage capacity, and is selected from graphite, hard carbon, porous carbon, or carbon nanotube materials.
[0025] In some embodiments, the vapor deposition is chemical vapor deposition (CVD) or plasma enhanced chemical vapor deposition (PECVD), with a temperature range of 300° C.-800° C. and a power of 100-500W.
[0026] In some embodiments, the silicon source is silane, and the nitrogen source is one or more of ammonia and nitrogen.
[0027] In some embodiments, the volume ratio of the silicon source to the nitrogen source is between 5 and 0.2.
[0028] In some embodiments, if the deposition method is chemical vapor deposition (CVD), the gas pressure ranges from 100-3000 Pa, and the temperature ranges from 400° C. to 600° C.
[0029] In some embodiments, if the deposition method is plasma enhanced chemical vapor deposition (PECVD), the gas pressure range is 0-100 Pa, the temperature range is 300° C.-600° C., and the power is 100-500W.
[0030] In some embodiments, a carbon substrate is placed in a tubular furnace, argon gas is introduced, and the temperature is raised to 300-800°C at 5°C / min. Then, a silicon source and a nitrogen source are introduced simultaneously in a certain proportion and a certain gas pressure is reached, and a SiNx composite silicon layer is obtained by vapor deposition.
[0031] The SiNx / Si composite silicon layer obtained by the above preparation method is characterized in that the internal structure is an inter-embedded structure of nano-SiNx and nano-silicon, wherein the nano-silicon particles are smaller than 5nm.
[0032] Figure 1 Schematic diagram of the structure of the silicon-carbon material containing the SiNx / Si composite silicon layer of the present invention. Figure 1 As shown, the circle in the center is carbon material, the ring is silicon material, and the small circle inside the ring is SiNx.
[0033] Example 1
[0034] The porous carbon material (specific surface area 1875m 2 / g) was placed in a tube furnace, argon was introduced, the temperature was raised to 500°C at a rate of 5°C / min, and then gas was introduced in a ratio of silane to ammonia of 5:1. When the gas pressure in the furnace tube reached 1300Pa, the timing was 20 minutes, and PC@SiNx / Si was deposited.
[0035] The SiNx / Si composite silicon layer obtained by the above preparation method is characterized in that the internal structure is an inter-embedded structure of nano-SiNx and nano-silicon, wherein the nano-silicon particles are smaller than 5nm.
[0036] The above silicon-carbon negative electrode material was prepared into a slurry according to the ratio of active material: Ketjen black: cmc: sbr = 8:1:0.5:0.5, and then coated on a 10-micron copper foil, vacuum dried for 12 hours and cut into 10 mm discs to obtain a silicon-carbon electrode, which was transferred to a super-purified glove box filled with argon gas to assemble a 2032-type button half-cell for testing, using a Celgard 2500 diaphragm and a metal lithium sheet as the counter electrode. The packaged button half-cell was left for 24 hours and then subjected to a constant current charge-discharge cycle test at a voltage range of 0.01-1.5V.
[0037] Example 2
[0038] The porous carbon material (specific surface area 1875m 2 / g) was placed in a tube furnace, argon was introduced, the temperature was raised to 500°C at a rate of 5°C / min, and then gas was introduced in a ratio of silane:ammonia of 3:1. When the gas pressure in the furnace tube reached 1300Pa, the timing was 20 minutes, and PC@SiNx / Si was deposited.
[0039] The SiNx / Si composite silicon layer obtained by the above preparation method is characterized in that the internal structure is an inter-embedded structure of nano-SiNx and nano-silicon, wherein the nano-silicon particles are smaller than 5nm.
[0040] The above silicon-carbon negative electrode material was prepared into a slurry according to the ratio of active material: Ketjen black: cmc: sbr = 8:1:0.5:0.5, and then coated on a 10-micron copper foil, vacuum dried for 12 hours and cut into 10 mm discs to obtain a silicon-carbon electrode, which was transferred to a super-purified glove box filled with argon gas to assemble a 2032-type button half-cell for testing, using a Celgard 2500 diaphragm and a metal lithium sheet as the counter electrode. The packaged button half-cell was left for 24 hours and then subjected to a constant current charge-discharge cycle test at a voltage range of 0.01-1.5V.
[0041] Example 3
[0042] The porous carbon material (specific surface area 1875m 2 / g) was placed in a tube furnace, argon was introduced, the temperature was raised to 500°C at a rate of 5°C / min, and then gas was introduced in a ratio of silane to ammonia of 1:1. When the gas pressure in the furnace tube reached 1300Pa, the timing was 20 minutes, and PC@SiNx / Si was deposited.
[0043] The SiNx / Si composite silicon layer obtained by the above preparation method is characterized in that the internal structure is an inter-embedded structure of nano-SiNx and nano-silicon, wherein the nano-silicon particles are smaller than 5nm.
[0044] The above silicon-carbon negative electrode material was prepared into a slurry according to the ratio of active material: Ketjen black: cmc: sbr = 8:1:0.5:0.5, and then coated on a 10-micron copper foil, vacuum dried for 12 hours and cut into 10 mm discs to obtain a silicon-carbon electrode, which was transferred to a super-purified glove box filled with argon gas to assemble a 2032-type button half-cell for testing, using a Celgard 2500 diaphragm and a metal lithium sheet as the counter electrode. The packaged button half-cell was left for 24 hours and then subjected to a constant current charge-discharge cycle test at a voltage range of 0.01-1.5V.
[0045] Example 4
[0046] The porous carbon material (specific surface area 1875m 2 / g) was placed in a tube furnace, argon was introduced, the temperature was raised to 500°C at a rate of 5°C / min, and then gas was introduced according to the ratio of silane:nitrogen of 2.5:1, the gas pressure was 50Pa, the RF power was 300W, the timing was 20min, and PC@SiNx / Si was deposited.
[0047] The SiNx / Si composite silicon layer obtained by the above preparation method is characterized in that the internal structure is an inter-embedded structure of nano-SiNx and nano-silicon, wherein the nano-silicon particles are smaller than 5nm.
[0048] The above silicon-carbon negative electrode material was prepared into a slurry according to the ratio of active material: Ketjen black: cmc: sbr = 8:1:0.5:0.5, and then coated on a 10-micron copper foil, vacuum dried for 12 hours and cut into 10 mm discs to obtain a silicon-carbon electrode, which was transferred to a super-purified glove box filled with argon gas to assemble a 2032-type button half-cell for testing, using a Celgard 2500 diaphragm and a metal lithium sheet as the counter electrode. The packaged button half-cell was left for 24 hours and then subjected to a constant current charge-discharge cycle test at a voltage range of 0.01-1.5V.
[0049] Example 5
[0050] The graphite material was placed in a tubular furnace, argon gas was introduced, the temperature was raised to 500°C at a rate of 5°C / min, and then gas was introduced in a ratio of silane:ammonia of 3:1. When the gas pressure in the furnace tube reached 1300Pa, the time was set for 20 minutes to deposit G@SiNx / Si.
[0051] The SiNx / Si composite silicon layer obtained by the above preparation method is characterized in that the internal structure is an inter-embedded structure of nano-SiNx and nano-silicon, wherein the nano-silicon particles are smaller than 5nm.
[0052] The above silicon-carbon negative electrode material was prepared into a slurry according to the ratio of active material: Ketjen black: cmc: sbr = 8:1:0.5:0.5, and then coated on a 10-micron copper foil, vacuum dried for 12 hours and cut into 10 mm discs to obtain a silicon-carbon electrode, which was transferred to a super-purified glove box filled with argon gas to assemble a 2032-type button half-cell for testing, using a Celgard 2500 diaphragm and a metal lithium sheet as the counter electrode. The packaged button half-cell was left for 24 hours and then subjected to a constant current charge-discharge cycle test at a voltage range of 0.01-1.5V.
[0053] Example 6
[0054] The multi-walled carbon nanotube material was placed in a tubular furnace, argon was introduced, the temperature was raised to 500°C at a rate of 5°C / min, and then gas was introduced in a ratio of silane:ammonia of 3:1. When the gas pressure in the furnace tube reached 1300Pa, the time was set for 20 minutes to deposit CNT@SiNx / Si.
[0055] The SiNx / Si composite silicon layer obtained by the above preparation method is characterized in that the internal structure is an inter-embedded structure of nano-SiNx and nano-silicon, wherein the nano-silicon particles are smaller than 5nm.
[0056] The above silicon-carbon negative electrode material was prepared into a slurry according to the ratio of active material: Ketjen black: cmc: sbr = 8:1:0.5:0.5, and then coated on a 10-micron copper foil, vacuum dried for 12 hours and cut into 10 mm discs to obtain a silicon-carbon electrode, which was transferred to a super-purified glove box filled with argon gas to assemble a 2032-type button half-cell for testing, using a Celgard 2500 diaphragm and a metal lithium sheet as the counter electrode. The packaged button half-cell was left for 24 hours and then subjected to a constant current charge-discharge cycle test at a voltage range of 0.01-1.5V.
[0057] Comparative Example 1
[0058] The porous carbon material (specific surface area 1875m 2 / g) was placed in a tube furnace, argon was introduced, the temperature was raised to 500°C at a rate of 5°C / min, and then silane was introduced. When the gas pressure in the furnace tube reached 1300 Pa, the time was set for 20 minutes to deposit and obtain a silicon-carbon composite material.
[0059] The above silicon-carbon negative electrode material was prepared into a slurry according to the ratio of active material: Ketjen black: cmc: sbr = 8:1:0.5:0.5, and then coated on a 10-micron copper foil, vacuum dried for 12 hours and cut into 10 mm discs to obtain a silicon-carbon electrode, which was transferred to a super-purified glove box filled with argon gas to assemble a 2032-type button half-cell for testing, using a Celgard 2500 diaphragm and a metal lithium sheet as the counter electrode. The packaged button half-cell was left for 24 hours and then subjected to a constant current charge-discharge cycle test at a voltage range of 0.01-1.5V.
[0060] Examples 1-3 are silicon-carbon negative electrode materials obtained by using silane and ammonia as silicon source and nitrogen source, and depositing them for the same time in different proportions. It can be seen from Table 1 that as the proportion of ammonia in the gas increases, the material capacity decreases significantly, 1982, 1628, 1201 mAh / g, all lower than Comparative Example 1, which is attributed to the generation of SiNx. Although the capacity of SiNx is much lower than that of silicon, it can greatly alleviate the volume expansion of the material, generate inorganic SEI components rich in nitrogen, and improve the cycle stability of the material. Therefore, after 250 cycles at 0.5C, Material Example 2 has a significantly higher capacity retention rate. Figure 3 This is the XRD image of Example 2 after being kept warm for 1 hour under argon protection at 800°C. The peak at 30-40° proves the presence of SiNx. The diffraction peak is still very wide after high-temperature crystallization, which is attributed to the fine grain widening effect. This shows that the particle size of the silicon particles is very small, and the material has a SiNx / Si nano-interlocking structure. According to the Scherrer formula, the grain size of the nano-silicon crystal is about 2nm. Example 4 uses a plasma enhanced chemical vapor deposition method to obtain a structure similar to that of Examples 1-3. Since some nitrogen sources such as nitrogen are difficult to decompose, the PECVD method can ensure the generation of SiNx under relatively mild conditions, which is more environmentally friendly than using ammonia as a nitrogen source. Examples 2, 5, and 6 are carbon SiNx / Si structures obtained after deposition of different carbon materials at the same ratio of silicon source and nitrogen source. Compared with materials with high specific surface area, materials obtained with graphite as the substrate have higher first efficiency and lower capacity. Carbon nanotubes have the highest capacity and excellent cycle performance, thanks to the properties of the carbon substrate. These examples demonstrate the universality of the silicon-carbon negative electrode material constructed by this method for carbon substrates.
[0061] Table 1 Comparison of electrochemical performance of Examples 1-6 and Comparative Example 1
[0062]
[0063] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a silicon-carbon material containing a SiNx / Si composite silicon layer, characterized in that: The carbon substrate is placed in a tubular furnace, and at a certain temperature, a silicon source and a nitrogen source are introduced simultaneously in a certain proportion and a certain gas pressure is reached, and a SiNx composite silicon layer is obtained by a vapor deposition method.
2. The method for preparing a silicon-carbon material containing a SiNx / Si composite silicon layer according to claim 1, characterized in that: The silicon layer contains Si3N4 ceramic phase and non-stoichiometric SiNx. The Si3N4 ceramic phase is not electrochemically active and, as an inert phase, alleviates the volume expansion of the silicon material during lithium insertion. The non-stoichiometric SiNx has a certain electrochemical activity and, while providing a certain capacity, promotes the formation of a nitrogen-containing SEI film and improves the lithium ion migration rate of the electrode. At the same time, during vapor deposition, the combination of nitrogen-containing radicals and silicon-containing radicals has a certain competitive effect with the bonding between silicon and silicon, reducing the particle size of the silicon particles and obtaining a SiNx / Si nano-intercalated structure. SiNx not only evenly disperses the nano-silicon particles, but also prevents electrochemical sintering during the material cycle, thereby improving the material's cycle performance.
3. The method for preparing a silicon-carbon material containing a SiNx / Si composite silicon layer according to claim 1, characterized in that: The carbon substrate has electrical conductivity and a certain lithium storage capacity, and is selected from graphite, hard carbon, porous carbon, or carbon nanotube materials.
4. The method for preparing a silicon-carbon material containing a SiNx / Si composite silicon layer according to claim 1, characterized in that: The vapor deposition is chemical vapor deposition (CVD) or plasma enhanced chemical vapor deposition (PECVD), with a temperature range of 300° C. to 800° C. and a power of 100 to 500W.
5. The method for preparing a silicon-carbon material containing a SiNx / Si composite silicon layer according to claim 1, characterized in that: The silicon source is silane, and the nitrogen source is one or more of ammonia and nitrogen.
6. The method for preparing a silicon-carbon material containing a SiNx / Si composite silicon layer according to claim 1, characterized in that: The volume ratio of the silicon source to the nitrogen source is between 5 and 0.
2.
7. The method for preparing a silicon-carbon material containing a SiNx / Si composite silicon layer according to claim 1, characterized in that: If the deposition method is chemical vapor deposition (CVD), the gas pressure range is 100-3000 Pa, and the temperature range is 400°C-600°C.
8. The method for preparing a silicon-carbon material containing a SiNx / Si composite silicon layer according to claim 1, characterized in that: If the deposition method is plasma enhanced chemical vapor deposition (PECVD), the gas pressure range is 0-100 Pa, the temperature range is 300° C.-600° C., and the power is 100-500W.
9. The method for preparing a silicon-carbon material containing a SiNx / Si composite silicon layer according to claim 1, characterized in that: The carbon substrate is placed in a tubular furnace, argon gas is introduced, and the temperature is raised to 300-800°C at 5°C / min. Then, a silicon source and a nitrogen source are introduced simultaneously in a certain proportion and a certain gas pressure is reached. A SiNx composite silicon layer is obtained by vapor deposition.
10. The composite silicon layer containing SiNx / Si obtained by the preparation method according to any one of claims 1 to 9, characterized in that: The internal structure is an inter-embedded structure of nano-SiNx and nano-silicon, in which the nano-silicon particles are less than 5nm.
Citation Information
Patent Citations
Negative material of lithium-ion battery and preparation method of negative material
CN103280581A
Negative electrode and method for manufacturing same
CN107851777A
Ceramic phase silicon-nitrogen layer coated silicon negative electrode material, preparation method and application of ceramic phase silicon-nitrogen layer coated silicon negative electrode material
CN114420912A
Application of nano silicon-nitrogen coated carbon composite material in negative electrode
CN114976012A
Preparation method of negative electrode material for long-cycle high-performance secondary battery and product thereof
CN116014087A