P-type organic material, self-driven gallium oxide ultraviolet photoelectric detector and preparation method thereof

By forming a PN heterojunction structure of p-type organic material on a β-Ga2O3 thin film layer, the problems of large size, easy damage and low responsivity of silicon-based solar-blind ultraviolet detectors are solved, realizing self-driven high-sensitivity ultraviolet photoelectric detection, which is suitable for high-temperature environments and reduces costs.

CN118908884AActive Publication Date: 2024-11-08HUBEI UNIV

Patent Information

Application Number
CN202410958170.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Existing silicon-based solar-blind ultraviolet photodetectors suffer from problems such as large size, easy damage, low responsivity, and poor high-temperature performance, and are also costly, making it difficult to meet the detection requirements of high sensitivity and high precision.

Method used

A self-driven PN heterojunction structure is formed by p-type organic materials and β-Ga2O3 thin film layers to reduce the operating voltage requirement. The high temperature tolerance and stability of gallium oxide are utilized, and a gold thin film layer is combined as a catalyst to promote the formation of β-Ga2O3 thin film layers.

Benefits of technology

It achieves high-sensitivity ultraviolet photodetector with self-drive under low voltage, reduces the system's weight and size, is suitable for high-temperature environments, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908884A_ABST
    Figure CN118908884A_ABST
Patent Text Reader

Abstract

The invention provides a p-type organic material, a self-driven gallium oxide ultraviolet photoelectric detector and a preparation method thereof. The self-driven gallium oxide ultraviolet photoelectric detector comprises a substrate; the gold film layer is located on the surface of the substrate; the beta-Ga2O3 thin film layer is located on the surface of the gold thin film layer; the organic material layer is located on the surface, away from the substrate, of the beta-Ga2O3 thin film layer, and the organic material layer incompletely covers the beta-Ga2O3 thin film layer; the first electrode is located on the surface of the organic material layer; the second electrode is positioned on the surface, which is not covered by the organic material layer, of the beta-Ga2O3 thin film layer; according to the invention, the novel P-type organic material layer is formed on one side of the beta-Ga2O3 thin film layer, so that a PN heterojunction structure which can respond to ultraviolet light to be self-driven is formed, and the voltage required by working is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ultraviolet photoelectric detectors, and in particular to a p-type organic material, a self-driven gallium oxide ultraviolet photoelectric detector and a preparation method thereof. Background Art

[0002] Due to the existence of the ozone layer, ultraviolet rays below 280nm in solar radiation can hardly reach the earth's surface, so the ultraviolet rays in the 200-280nm band are called the solar-blind ultraviolet region. The background noise of ultraviolet radiation in the solar-blind region is small, so detectors based on this band have the characteristics of high sensitivity and high precision. Ultraviolet detection technology is of great significance in military fields such as ultraviolet communication, ultraviolet guidance, and missile warning. It also has broad application prospects in people's livelihood fields such as high-response fire warning, atmospheric environment monitoring, and cell cancer detection.

[0003] At present, the practical solar-blind ultraviolet photodetectors are mainly silicon-based photomultiplier tubes and silicon-based ultraviolet detectors, but these two silicon-based devices have some shortcomings: photomultiplier tubes need to work under high voltage, have large volume and mass, are easily damaged, and are not easy to integrate; silicon-based ultraviolet detectors need additional filters to filter out light other than the target wavelength, and have low responsivity and poor high-temperature performance. Therefore, it is necessary to develop new materials and new solar-blind ultraviolet detectors.

[0004] A variety of ultra-wide bandgap semiconductor materials with band gaps corresponding to the solar-blind zone are used to prepare solar-blind ultraviolet photodetectors. Solar-blind ultraviolet detectors based on ultra-wide bandgap semiconductor materials can work in the solar-blind band without the need for external filters, which helps to simplify the deep ultraviolet detection system and can effectively reduce the mass and volume of the system. Currently, materials such as MgZnO and AlGaN used in the research of solar-blind ultraviolet photodetectors require precise control of conditions such as composition and temperature, and are relatively expensive. In contrast, gallium oxide has the following advantages for ultraviolet detection: the bandgap width of gallium oxide (4.4-5.3eV) directly corresponds to the solar-blind band; gallium oxide has a high tolerance to high temperature, high pressure, and strong radiation environments, and has stable physical and chemical properties; gallium oxide single crystal substrates can be obtained by melting method, and the production cost is relatively low, which is conducive to large-scale mass production; gallium oxide and gallium are easy to process and are considered to be a very promising ultraviolet detection material.

[0005] Therefore, it is of great significance to research, develop and design different types of ultraviolet photodetectors so that they can be widely used in different fields. Summary of the invention

[0006] In view of this, the present invention provides a p-type organic material, a self-driven gallium oxide ultraviolet photodetector and a preparation method thereof to solve the defects existing in the prior art.

[0007] In a first aspect, the present invention provides a p-type organic material, the chemical structure of the p-type organic material is as follows:

[0008]

[0009] Wherein, R4, R5, and R6 are each independently selected from any one of the following groups:

[0010]

[0011] Preferably, the chemical structure of the p-type organic material is as follows:

[0012]

[0013] In a second aspect, the present invention further provides a self-driven gallium oxide ultraviolet photodetector, comprising:

[0014] substrate;

[0015] A gold thin film layer, which is located on the surface of the substrate;

[0016] A β-Ga2O3 thin film layer, which is located on the surface of the gold thin film layer away from the substrate;

[0017] An organic material layer, which is located on a surface of the β-Ga2O3 thin film layer away from the substrate, and the organic material layer does not completely cover the β-Ga2O3 thin film layer;

[0018] A first electrode, which is located on a surface of the organic material layer away from the substrate;

[0019] A second electrode, which is located on the surface of the β-Ga2O3 thin film layer not covered by the organic material layer;

[0020] Wherein, the material of the organic material layer is the p-type organic material.

[0021] Preferably, the thickness of the gold thin film layer is 30 to 60 nm;

[0022] and / or, the thickness of the β-Ga2O3 thin film layer is 0.5 to 1 μm;

[0023] And / or, the thickness of the organic material layer is 50-1000 nm.

[0024] Preferably, the material used for the first electrode and the second electrode includes at least one of Cu, Pt, Au, Al, and Ni.

[0025] Preferably, the substrate includes any one of a sapphire substrate, a silicon substrate, a quartz substrate, and a MgO substrate.

[0026] In a third aspect, the present invention further provides a method for preparing the self-driven gallium oxide ultraviolet photodetector, comprising the following steps:

[0027] Preparing a gold thin film layer on the surface of the substrate;

[0028] Prepare a β-Ga2O3 thin film layer on the surface of the gold thin film layer;

[0029] Preparing an organic material layer on the surface of the β-Ga2O3 thin film layer, wherein the organic material layer does not completely cover the β-Ga2O3 thin film layer;

[0030] Prepare a first electrode on the surface of the organic material layer;

[0031] A second electrode is prepared on the surface of the β-Ga2O3 thin film layer covered by the organic material layer.

[0032] Preferably, preparing the β-Ga2O3 thin film layer on the surface of the gold thin film layer specifically includes:

[0033] Ga metal is used as a gallium source and then placed at one end of the tube furnace where the gas is introduced;

[0034] The substrate with the gold film evaporated thereon is then placed in a tubular furnace 5-10 cm away from a gallium source and subjected to high temperature treatment in an inert atmosphere to obtain a β-Ga2O3 thin film layer.

[0035] Preferably, the high temperature treatment temperature is 700-1000°C and the time is 1-3h;

[0036] The inert atmosphere includes at least one of nitrogen, helium, neon and argon.

[0037] Preferably, the gold thin film layer is prepared by evaporation, wherein the process parameters during evaporation are: the pressure of the evaporator cavity is (5-9)×10 -4 Pa, the current is 100-140A, and the evaporation time is 30-60min.

[0038] Preferably, preparing the organic material layer on the surface of the β-Ga2O3 thin film layer specifically includes:

[0039] Adding a p-type organic material into chlorobenzene to prepare an organic material solution;

[0040] The organic material solution is coated on the surface of the β-Ga2O3 thin film layer and dried to obtain the organic material layer.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] 1. The p-type organic material of the present invention can be used to form a PN heterojunction structure with a β-Ga2O3 thin film layer that can be self-driven in response to ultraviolet light, effectively reducing the voltage required for operation;

[0043] 2. The self-driven gallium oxide ultraviolet photodetector of the present invention forms a new type of P-type organic material layer on one side of the β-Ga2O3 thin film layer to form a PN heterojunction structure that can be self-driven in response to ultraviolet light, thereby effectively reducing the voltage required for operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the prior art descriptions. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0045] Figure 1 is the hydrogen nuclear magnetic resonance spectrum of compound 3 in Example 1 of the present invention;

[0046] Figure 2 is the hydrogen nuclear magnetic resonance spectrum of compound 5 in Example 1 of the present invention;

[0047] Figure 3 It is a schematic structural diagram of the self-driven gallium oxide ultraviolet photodetector of the present invention;

[0048] Figure 4 The photocurrent rise and fall curves of the self-driven gallium oxide ultraviolet photodetector under 0V bias in Example 2 of the present invention;

[0049] Figure 5 1 is a light / dark state IV curve of the self-driven gallium oxide ultraviolet photodetector in Example 2 of the present invention. DETAILED DESCRIPTION

[0050] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. In addition, in the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may be in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single values ​​within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the numbered ranges, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any quoted numbers (fractions or integers) within the indicated range.

[0052] The present application embodiment provides a p-type organic material, whose chemical structure is as follows:

[0053]

[0054] Wherein, R4, R5, and R6 (the wavy shapes in R4, R5, and R6 indicate the positions where R4, R5, and R6 are connected to the main structure of the p-type organic material) are independently selected from any one of the following groups:

[0055]

[0056] Preferably, in some embodiments, R4, R5, and R6 are At this time, the chemical structure of the p-type organic material is as follows:

[0057]

[0058] Furthermore, the synthesis route of the p-type organic material (i.e., compound 5) of the present invention is as follows:

[0059]

[0060] Wherein, the R1 group in Compound 1, Compound 2 and Compound 3 is selected from any one of -X, -COOH, =O, -CH3, -H, -CH2CH3; X is a halogen, specifically any one of F, Cl, Br, I;

[0061] The R2 group of compound 2 is selected from -CH2CH3, -OH, =O, -COOH, -OC n H n+2 , -CH3, -H; n is a positive integer between 1 and 20.

[0062] The R3 group of compound 4 is selected from any one of the following groups:

[0063] Wherein, R is independently selected from any one of -Cl, -Br, and -I; and R in the R3 group is connected to the N atom of compound 4.

[0064] Preferably, the chemical structural formula of compound 1 is: The chemical structure of compound 2 is The chemical structure of compound 3 is The structural formula of compound 4 is

[0065] Specifically, the synthesis method of compound 3 is:

[0066] Compound 1 (0.5-1.0 g), ethanol or methanol (5-25 mL), and potassium salt (0.38 g, specifically potassium tert-butoxide (t-BuOK)) were added to a two-necked flask, and heated to reflux at 130° C. for 40-80 minutes under nitrogen protection; then compound 2 (0.45 g) was added to the reaction system, and reflux was continued for 20-30 minutes; the reaction system was cooled and poured into 200-500 mL of water, solid matter precipitated, and an appropriate amount of hydrochloric acid was added to neutralize the mixture to neutrality; finally, the precipitate was filtered and dried, and the crude product was washed 3 times to obtain a yellow powder, namely compound 3.

[0067] The synthesis method of compound 5 (i.e., the p-type organic material of the present invention) is:

[0068] Compound 3 (0.1-0.2 g), compound 4 (0.7-0.8 g), tetrakis(triphenylphosphine)palladium (0.02-0.07 g), N,N-dimethylformamide (15-25 mL), 2M potassium salt aqueous solution (1-1.3 g, specifically 2 mol / L potassium carbonate aqueous solution) were added to a two-necked flask, heated to 90°C under nitrogen protection, and stirred for 20 hours. After the reaction was completed, the mixture in the flask was cooled to room temperature and poured into a cold sodium sulfate aqueous solution, stirred until the precipitate was completely precipitated, the solid was filtered out and dried to obtain a crude product, and purified to obtain an orange-red solid, which was compound 5.

[0069] Based on the same inventive concept, the present invention also provides a self-driven gallium oxide ultraviolet photodetector, such as Figure 3 As shown, including:

[0070] Base 1;

[0071] A gold thin film layer 2, which is located on the surface of the substrate 1;

[0072] β-Ga2O3 thin film layer 3, which is located on the surface of the gold thin film layer 2 away from the substrate 1;

[0073] An organic material layer 4 is located on a surface of the β-Ga2O3 thin film layer 3 away from the substrate 1, and the organic material layer 4 does not completely cover the β-Ga2O3 thin film layer 3;

[0074] A first electrode 5, which is located on a surface of the organic material layer 4 away from the substrate 1;

[0075] A second electrode 6, which is located on the surface of the β-Ga2O3 thin film layer 3 and not covered by the organic material layer 4;

[0076] The material of the organic material layer 4 is the above-mentioned p-type organic material.

[0077] The self-driven gallium oxide ultraviolet photodetector of the present invention comprises a substrate 1, a gold thin film layer 2 located on the surface of the substrate 1, a β-Ga2O3 thin film layer 3 located on the surface of the gold thin film layer 2, an organic material layer 4 located on the surface of the β-Ga2O3 thin film layer 3, a first electrode 5, and a second electrode 6; wherein the area of ​​the organic material layer 4 is smaller than the area of ​​the β-Ga2O3 thin film layer 3, so that the organic material layer 4 does not completely cover the β-Ga2O3 thin film layer 3, that is, a portion of the β-Ga2O3 thin film layer 3 is exposed; the first electrode 5 is located on the surface of the organic material layer 4 The second electrode 6 is located on the surface of the β-Ga2O3 thin film layer 3 that is not covered by the organic material layer 4, that is, the second electrode 6 is located on the exposed surface of the β-Ga2O3 thin film layer 3; wherein the gold thin film layer 2 serves as a catalyst for growing the β-Ga2O3 thin film layer 3, which can promote the formation of the β-Ga2O3 thin film layer 3 and improve the quality of the β-Ga2O3 thin film layer 3; the β-Ga2O3 thin film layer 3, as a photosensitive layer, is suitable for responding to ultraviolet light to output electrical signals; the organic material layer 4 is suitable for forming a PN heterojunction with the β-Ga2O3 thin film layer 3. The self-driven gallium oxide ultraviolet photodetector of the present invention is a two-terminal device, and the first electrode and the second electrode serve as an anode and a cathode respectively.

[0078] The self-driven gallium oxide ultraviolet photodetector of the present invention forms a novel P-type organic material layer on one side of the β-Ga2O3 thin film layer to form a PN heterojunction structure that can be self-driven in response to ultraviolet light, thereby effectively reducing the voltage required for operation.

[0079] In some embodiments, the thickness of the gold thin film layer 2 is 30-60 nm.

[0080] In some embodiments, the thickness of the β-Ga2O3 thin film layer 3 is 0.5-1 μm.

[0081] In some embodiments, the thickness of the organic material layer 4 is 50-1000 nm.

[0082] In some embodiments, the material used for the first electrode 5 and the second electrode 6 includes at least one of Cu, Pt, Au, Al, and Ni.

[0083] In some embodiments, the substrate 1 includes any one of a sapphire substrate, a silicon substrate, a quartz substrate, and a MgO substrate.

[0084] Based on the same inventive concept, the present invention also provides a method for preparing the above-mentioned self-driven gallium oxide ultraviolet photodetector, comprising the following steps:

[0085] S1, preparing a gold thin film layer on the surface of the substrate;

[0086] S2, preparing a β-Ga2O3 thin film layer on the surface of the gold thin film layer;

[0087] S3, preparing an organic material layer on the surface of the β-Ga2O3 thin film layer, wherein the organic material layer does not completely cover the β-Ga2O3 thin film layer;

[0088] S4, preparing a first electrode on the surface of the organic material layer;

[0089] S5. Prepare a second electrode on the surface of the β-Ga2O3 thin film layer covered by the organic material layer.

[0090] In some embodiments, preparing a β-Ga2O3 thin film layer on the surface of the gold thin film layer specifically includes:

[0091] Ga metal is used as a gallium source and then placed at one end of the tube furnace where the gas is introduced;

[0092] The substrate with the gold film deposited thereon is then placed in a tubular furnace 5 to 10 cm away from a gallium source and treated at high temperature in an inert atmosphere to obtain a β-Ga2O3 thin film layer.

[0093] In some embodiments, the high temperature treatment temperature is 700-1000° C. and the time is 1-3 hours.

[0094] In some embodiments, the inert atmosphere includes at least one of nitrogen, helium, neon, and argon.

[0095] In some embodiments, the gold thin film layer is prepared by evaporation, wherein the process parameters during evaporation are: the pressure of the evaporator chamber is (5-9)×10 -4 Pa, the current is 100-140A, and the evaporation time is 30-60min.

[0096] In some embodiments, preparing an organic material layer on the surface of the β-Ga2O3 thin film layer specifically includes:

[0097] Adding a p-type organic material into an organic solvent to prepare an organic material solution;

[0098] The organic material solution is coated on the surface of the β-Ga2O3 thin film layer and dried to obtain the organic material layer.

[0099] Specifically, the organic solvent is chlorobenzene.

[0100] In some embodiments, the first electrode and the second electrode are prepared by magnetron sputtering, evaporation, or the like.

[0101] Specifically, in some embodiments, a method for preparing a self-driven gallium oxide ultraviolet photodetector comprises the following steps:

[0102] S1. Clean the substrate. The cleaning process is as follows: soak the substrate in deionized water, acetone, and anhydrous ethanol in turn, and ultrasonicate for 20 minutes each. After taking it out, rinse it with deionized water, and finally dry it in a drying oven for standby use.

[0103] S2, fix the substrate on the fixing frame of the evaporator, place two gold particles in the tungsten boat, then evacuate the chamber of the evaporator to vacuum, evaporate a layer of gold film on the substrate, obtain a gold film layer / substrate, and set it aside;

[0104] S3, using Ga metal as a gallium source, and then placing it at one end of the tube furnace where the gas is introduced;

[0105] S4, placing the substrate with the gold film evaporated thereon in a tube furnace 5 to 10 cm away from the gallium source, and subjecting it to high temperature treatment in an inert atmosphere to obtain a β-Ga2O3 thin film layer;

[0106] S5, introducing argon gas into the tubular furnace, evacuating and ventilating for more than three times to ensure that the quartz tube of the tubular furnace is filled with argon gas atmosphere, and then starting the tubular furnace to perform high temperature treatment of Ga metal / gold thin film layer / substrate to obtain β-Ga2O3 thin film layer / gold thin film layer / substrate for standby use;

[0107] S6, cleaning the sample bottle and the magnetic rotor, immersing the sample bottle and the magnetic rotor in deionized water, acetone, and anhydrous ethanol in turn, ultrasonically for 20 minutes each, taking them out and then rinsing them with deionized water, and finally drying them in a drying oven for standby use;

[0108] S7. In a glove box, an organic material solution is prepared in a sample bottle, the solvent is chlorobenzene (i.e., p-type organic material is added to chlorobenzene to prepare an organic material solution), first, a portion of the β-Ga2O3 film layer / gold film layer / substrate is covered with a gold finger tape, and the substrate is placed in an ultraviolet ozone cleaning machine for 30 minutes to make the substrate more adsorbent and convenient for spin coating; 20 to 40 μL of the organic material solution is taken out with a pipette and dropped on one side of the β-Ga2O3 film layer / gold film layer / substrate, the β-Ga2O3 film layer / gold film layer / substrate is fixed on a spin coater, the spin coater is turned on, and the organic material is evenly spin-coated on the portion not covered with the gold finger tape, so that the organic material forms an organic / inorganic heterojunction with the β-Ga2O3 film layer on one side, and an organic material layer / β-Ga2O3 film layer / gold film layer / substrate is obtained, and the organic material layer / β-Ga2O3 film layer / gold film layer / substrate is set aside;

[0109] S8. Use gold finger tape to fix the mask on the surface of the organic material layer / β-Ga2O3 thin film layer / gold thin film layer / substrate, so that the two holes of the mask are aligned with the organic material layer and the β-Ga2O3 thin film layer. Fix the substrate on the fixing frame of the evaporator, place the metal required for the first electrode in the tungsten boat, then evacuate the cavity of the evaporator to vacuum, evaporate the first electrode on the organic material layer / β-Ga2O3 thin film layer / gold thin film layer / substrate, use the same method to make the second electrode, and obtain the entire device.

[0110] Specifically, in the above steps S2 and S8, the pressure of the vacuum chamber for evaporating the gold film is adjusted to 7×10 -4 Pa, the current is 100-140A, and the evaporation time is 30-60min.

[0111] In the above step S5, the temperature of the high temperature treatment of Ga metal and gold thin film layer / substrate is 700° C. to 1000° C., the duration is 1 to 3 hours, and the gas atmosphere is an argon atmosphere.

[0112] The following further describes the self-driven gallium oxide ultraviolet photodetector and its preparation method of the present application with specific examples. This section further describes the content of the present invention in conjunction with specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0113] Example 1

[0114] This embodiment provides a p-type organic material, whose chemical structure is as follows:

[0115]

[0116] Specifically, the synthesis route of the above-mentioned p-type organic material (i.e., compound 5) is as follows:

[0117]

[0118] The synthesis method of compound 3 is as follows:

[0119] 2,7-Dibromofluorene (i.e., compound 1, 2.5mmol, 0.8g), anhydrous ethanol (15mL), and potassium tert-butoxide (0.38g) were added to a 100mL two-necked flask, and heated to reflux at 130°C for 60 minutes under nitrogen protection; then 2-bromo-5-formylpyridine (i.e., compound 2, 2.4mmol, 0.45g) was added to the reaction system, and reflux was continued for 20 minutes; after the reaction was completed, the reaction system was cooled and poured into 200mL of water, solid matter precipitated, and an appropriate amount of concentrated hydrochloric acid was added to neutralize the mixture to neutrality. Finally, the precipitate was filtered and dried, and the crude product was washed with ethanol three times to obtain a yellow powder (1.1g, yield 90%), which was compound 3; the nuclear magnetic resonance hydrogen spectrum of compound 3 is as follows Figure 1 As shown; 1 H NMR(500MHz,DMSO-d6)δ8.63(d,J=2.4Hz,1H),8.25(d,J=1.7Hz,1H),8.05-7.9 8(m,2H),7.92-7.84(m,3H),7.63(td,J=8.3,1.7Hz,2H),7.43(d,J=1.6Hz,1H).

[0120] The synthesis method of compound 5 is as follows:

[0121] Compound 3 (0.35mmol, 0.17g), compound 4 (1.75mmol, 0.75g), tetrakis(triphenylphosphine)palladium (0.05mmol, 0.057g), N,N-dimethylformamide (20mL), 2M potassium carbonate aqueous solution (8mmol, 1.1g) were added to a 100mL two-necked flask, heated to 90°C under nitrogen protection, and stirred for 20 hours; after the reaction was completed, the mixture in the flask was cooled to room temperature and poured into 300mL of cold sodium sulfate aqueous solution, stirred thoroughly until the precipitate was completely precipitated, and the solid was filtered out and dried to obtain a crude product. The crude product was purified by column chromatography (dichloromethane as eluent) to obtain an orange-red solid (299mg, yield 73%), which was compound 5 (i.e., the p-type organic material of the present invention); the nuclear magnetic resonance hydrogen spectrum of compound 5 is as follows Figure 2 As shown; 1HNMR(500MHz,DMSO-d6)δ8.83(d,J=1.9Hz,1H),8.25(s,1H),8.11(dd,J=8.3,2.0Hz ,1H),8.06(s,1H),7.97(m,3H),7.89(dd,J=7.9,6.2Hz,2H),7.73-7.63(m,4H),7.58 (d,J=8.0,1H),7.28(d,J=8.7Hz,2H),7.10-7.04(m,8H),7.01-6.93(m,12H),6.90-6 .85(m,6H),6.80(d,J=8.8Hz,2H),6.72(d,J=8.6Hz,2H),3.76(s,12H),3.71(s,6H).

[0122] Example 2

[0123] This embodiment also provides a self-driven gallium oxide ultraviolet photodetector, including:

[0124] substrate;

[0125] a gold thin film layer, which is located on the surface of the substrate;

[0126] β-Ga2O3 thin film layer, which is located on the surface of the gold thin film layer away from the substrate;

[0127] An organic material layer is located on a surface of the β-Ga2O3 thin film layer away from the substrate, and the organic material layer does not completely cover the β-Ga2O3 thin film layer;

[0128] A first electrode, which is located on a surface of the organic material layer away from the substrate;

[0129] A second electrode, which is located on a surface of the β-Ga2O3 thin film layer that is not covered by the organic material layer;

[0130] Wherein, the material of the organic material layer is the p-type organic material in the above-mentioned embodiment 1;

[0131] The thickness of the gold film layer is 45 nm;

[0132] The thickness of the β-Ga2O3 thin film layer is 0.7 μm;

[0133] The thickness of the organic material layer is 200 nm;

[0134] The materials used for the first electrode and the second electrode are both gold;

[0135] The substrate is a sapphire substrate.

[0136] This embodiment also provides a method for preparing the above-mentioned self-driven gallium oxide ultraviolet photodetector, comprising the following steps:

[0137] S1. Clean the substrate. The cleaning process is as follows: soak the substrate in deionized water, acetone, and anhydrous ethanol in turn, and ultrasonicate for 20 minutes each. After taking it out, rinse it with deionized water, and finally dry it in a drying oven for standby use.

[0138] S2, fix the substrate on the fixing frame of the evaporator, place two gold particles in the tungsten boat, then evacuate the chamber of the evaporator to vacuum, evaporate a layer of gold film on the substrate, obtain a gold film layer / substrate, and set it aside;

[0139] S3, using Ga metal as a gallium source, and then placing it at one end of the tube furnace where the gas is introduced;

[0140] S4, placing the gold thin film layer / substrate with the gold thin film evaporated thereon in a tube furnace at a distance of 5-10 cm from the gallium source, and subjecting it to high temperature treatment under an inert atmosphere to obtain a β-Ga2O3 thin film layer;

[0141] S5, introducing argon gas into the tubular furnace, evacuating and ventilating for more than three times to ensure that the quartz tube of the tubular furnace is filled with argon gas atmosphere, and then opening the tubular furnace to treat Ga metal and gold thin film layer / substrate at high temperature to obtain β-Ga2O3 thin film layer / gold thin film layer / substrate for standby use;

[0142] S6, cleaning the sample bottle and the magnetic rotor, immersing the sample bottle and the magnetic rotor in deionized water, acetone, and anhydrous ethanol in turn, ultrasonically for 20 minutes each, taking them out and then rinsing them with deionized water, and finally drying them in a drying oven for standby use;

[0143] S7. Prepare an organic material solution in a sample bottle in a glove box (specifically, add p-type organic material to chlorobenzene to obtain an organic material solution with a concentration of 1 mg / mL). The solvent is chlorobenzene. First, use gold finger tape to cover a portion of the β-Ga2O3 film layer / gold film layer / substrate. Place the substrate in a UV ozone cleaner for 30 minutes to make the substrate more adsorbent and easy to spin coat. Use a pipette to take out 20 to 40 μL of organic material solution and drop it on one side of the β-Ga2O3 film layer / gold film layer / substrate. Fix the β-Ga2O3 film layer / gold film layer / substrate on a spin coater, turn on the spin coater, and evenly spin coat the organic material on the part not covered by the gold finger tape, so that the organic material forms an organic / inorganic heterojunction with the β-Ga2O3 film layer on one side, and obtain an organic material layer / β-Ga2O3 film layer / gold film layer / substrate for standby use.

[0144] S8. Use gold finger tape to fix the mask on the surface of the organic material layer / β-Ga2O3 thin film layer / gold thin film layer / substrate, so that the two holes of the mask are just aligned with the organic material layer and the β-Ga2O3 thin film layer, fix the substrate on the fixing frame of the evaporator, place the metals required for the first electrode and the second electrode in the tungsten boat, then evacuate the cavity of the evaporator to vacuum, evaporate the first electrode and the second electrode on the organic material layer / β-Ga2O3 thin film layer / gold thin film layer / substrate to obtain the entire device.

[0145] In the above step S2, the pressure of the vacuum chamber for evaporating the gold film is adjusted to 7×10 -4 Pa, the current is 120A;

[0146] In the above step S5, the temperature of the high temperature treatment of Ga metal and gold thin film layer / substrate is 900° C., the duration is 2 hours, and the gas atmosphere is argon atmosphere.

[0147] Performance Testing

[0148] Figure 4 The photocurrent rise and fall curves of the self-driven gallium oxide ultraviolet photodetector under 0V bias in Example 1 of the present invention;

[0149] Figure 5 1 is a light / dark state IV curve of the self-driven gallium oxide ultraviolet photodetector in Example 1 of the present invention.

[0150] refer to Figure 4 , Figure 5 As shown, under the condition of 0V bias, the embodiment of the present invention still has obvious light-dark current comparison, indicating that under the device structure of the present invention, the device has self-driving performance.

[0151] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A p-type organic material, characterized in that: The chemical structural formula of the p-type organic material is as follows: Wherein, R4, R5, and R6 are each independently selected from any one of the following groups:

2. The p-type organic material according to claim 1, characterized in that The chemical structure of the p-type organic material is shown below:

3. A self-driven gallium oxide ultraviolet photodetector, characterized in that: include: substrate; A gold thin film layer, which is located on the surface of the substrate; A β-Ga2O3 thin film layer, which is located on the surface of the gold thin film layer away from the substrate; An organic material layer, which is located on a surface of the β-Ga2O3 thin film layer away from the substrate, and the organic material layer does not completely cover the β-Ga2O3 thin film layer; A first electrode, which is located on a surface of the organic material layer away from the substrate; A second electrode, which is located on the surface of the β-Ga2O3 thin film layer not covered by the organic material layer; Wherein, the material of the organic material layer is the p-type organic material as claimed in claim 1 or 2.

4. The self-driven gallium oxide ultraviolet photodetector according to claim 3, characterized in that: The thickness of the gold thin film layer is 30 to 60 nm; and / or, the thickness of the β-Ga2O3 thin film layer is 0.5 to 1 μm; And / or, the thickness of the organic material layer is 50-1000 nm.

5. The self-driven gallium oxide ultraviolet photodetector according to claim 3, characterized in that: The material used for the first electrode and the second electrode includes at least one of Cu, Pt, Au, Al, and Ni; And / or, the substrate includes any one of a sapphire substrate, a silicon substrate, a quartz substrate, and a MgO substrate.

6. A method for preparing a self-driven gallium oxide ultraviolet photodetector according to any one of claims 3 to 5, characterized in that: The following steps are involved: Preparing a gold thin film layer on the surface of the substrate; Prepare a β-Ga2O3 thin film layer on the surface of the gold thin film layer; Preparing an organic material layer on the surface of the β-Ga2O3 thin film layer, wherein the organic material layer does not completely cover the β-Ga2O3 thin film layer; Prepare a first electrode on the surface of the organic material layer; A second electrode is prepared on the surface of the β-Ga2O3 thin film layer covered by the organic material layer.

7. The method for preparing the self-driven gallium oxide ultraviolet photodetector according to claim 6, characterized in that: The preparation of the β-Ga2O3 thin film layer on the surface of the gold thin film layer specifically includes: Ga metal is used as a gallium source and then placed at one end of the tube furnace where the gas is introduced; The substrate with the gold film deposited thereon is then placed in a tubular furnace 5 to 10 cm away from a gallium source and treated at high temperature in an inert atmosphere to obtain a β-Ga2O3 thin film layer.

8. The method for preparing the self-driven gallium oxide ultraviolet photodetector according to claim 7, characterized in that: The high temperature treatment temperature is 700-1000°C and the time is 1-3h; The inert atmosphere includes at least one of nitrogen, helium, neon and argon.

9. The method for preparing the self-driven gallium oxide ultraviolet photodetector according to claim 6, characterized in that: The gold thin film layer was prepared by evaporation method, wherein the process parameters during evaporation were: the pressure of the evaporator chamber was (5-9)×10 -4 Pa, the current is 100-140A, and the evaporation time is 30-60min.

10. The method for preparing the self-driven gallium oxide ultraviolet photodetector according to claim 6, characterized in that: The preparation of the organic material layer on the surface of the β-Ga2O3 thin film layer specifically includes: Adding a p-type organic material into chlorobenzene to prepare an organic material solution; The organic material solution is spin-coated on the surface of the β-Ga2O3 thin film layer and dried to obtain the organic material layer.

Citation Information

Patent Citations

  • PN junction structure based on gallium oxide and preparation method thereof

    CN111063742A

  • P-type gallium oxide thin film and preparation method and application thereof

    CN117071071A

  • Double-junction coupling type self-driven ultraviolet photoelectric detector and preparation method thereof

    CN117476790A

  • Method of manufacturing p-type gallium oxide by intrinsic doping, the thin film obtained from gallium oxide and its use

    US20200350166A1

Cited By