Inorganic-organic hybrid photoelectrochromic material as well as preparation method and application thereof
Through the solvent thermal synthesis method of inorganic-organic hybrid photoelectrochromic materials, the problem of slow response rate of photochromic materials is solved, and the rapid and reversible photochromic performance is achieved, which is suitable for a variety of application fields.
Patent Information
- Application Number
- CN202410944798.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-15
AI Technical Summary
Existing photochromic materials have problems such as single stimulation response, single application mode, and slow response rate.
Inorganic-organic hybrid photoelectrochromic materials are used, with the specific chemical formula C36H20N6O18Zn3, and by solvent heat The synthetic method is prepared to form a monoclinic crystal with a blocky crystal system, which has fast and reversible photochromic properties.
It has achieved the change from colorless to light blue within 10 s under ultraviolet light, and after 30 s, it has achieved a blue visible to the naked eye, with a significantly improved response rate, and ink-free printing, electrochromic devices, photochromic decoration, and optical memory. , optical switches and photoelectric display fields have wide application prospects.
Smart Images

Figure CN118908983A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photoelectric color change, and in particular to an inorganic-organic hybrid photoelectric color change material based on 2,4,6-tris(4-pyridyl)-1,3,5-triazine, and a preparation method and application thereof. Background Art
[0002] Photochromic compounds refer to compounds that change color under the action of light of a certain wavelength and intensity, and this change is reversible. Due to the characteristic of reversible switching between two different stable states, this type of material has been used in many fields, such as inks, automobiles, molecular switches, radiation detection, biological imaging, etc., showing broad application prospects.
[0003] Photochromic materials are divided into inorganic photochromic materials, organic photochromic materials, and inorganic-organic hybrid photochromic materials. Inorganic photochromic compounds include polyacids, alkali metal azides, valence tautomerism Prussian blue compounds, etc.; organic photochromic compounds include diarylethenes, spiropyrans, spirooxazines, azo compounds, viologens, etc. Inorganic compounds are thermally stable, while organic compounds are of many types and easy to process. Inorganic-organic hybrid materials combine the advantages of inorganic photochromic compounds and organic photochromic compounds. The research on inorganic-organic hybrid materials in photochromism has aroused great research interest.
[0004] Electrochromic devices refer to devices whose transmittance or reflectance undergoes a reversible optical change when an external voltage is applied. Due to their unique adjustable optical properties, electrochromic devices have attracted extensive attention in the fields of smart windows, sensors, and displays.
[0005] However, due to the late start of the development of this type of material, the current research on photochromic materials still has problems such as single stimulus response, single application mode and slow response rate. Summary of the invention
[0006] In order to solve the problems of single stimulus response, single application mode and slow response rate, the present invention provides an inorganic-organic hybrid photoelectric chromic material and a preparation method and application thereof.
[0007] The present invention adopts the following technical solutions:
[0008] An inorganic-organic hybrid photoelectric chromic material, wherein the chemical formula of the hybrid photoelectric chromic material is C 36 H 20 N6O 18 Zn3, the inorganic part is Zn 2+The organic part is 2,4,6-tris(4-pyridyl)-1,3,5-triazine and trimesic acid, monoclinic system, space group P21 / n, unit cell parameters are α=90°, β=95.60(3)°, γ=90°.
[0009] A preparation method of an inorganic-organic hybrid photoelectric chromic material comprises the following steps: uniformly mixing a metal source, 2,4,6-tris(4-pyridyl)-1,3,5-triazine (TPT for short), trimesic acid (BTC for short), water, N,N′-dimethylacetamide (DMA for short) and methanol to obtain a mixture, and charging the mixture into a reaction container for reaction to obtain block-shaped colorless crystals, namely the hybrid photoelectric chromic material.
[0010] Furthermore, the metal source is zinc perchlorate Zn(ClO4)2.
[0011] Furthermore, the mass ratio of the metal source, 2,4,6-tris(4-pyridyl)-1,3,5-triazine and trimesic acid is (2-4):1:(1-2), preferably 3:1:2.
[0012] Furthermore, the volume ratio of water, N,N′-dimethylacetamide and methanol is 4:1:(0-1), preferably 4:1:1.
[0013] Furthermore, the reaction temperature of the mixture is 120-140° C., preferably 140° C., and the reaction time is 24-72 hours.
[0014] Furthermore, the preparation method of the hybrid photoelectric induced chromic material comprises the following steps: 30 mg of zinc perchlorate, 10 mg of 2,4,6-tris(4-pyridyl)-1,3,5-triazine, 20 mg of trimesic acid, 4 mL of water, 1 mL of N,N′-dimethylacetamide, and 1 mL of methanol are uniformly mixed to obtain a mixture, and then added into a stainless steel reactor lined with polytetrafluoroethylene (the volume of the stainless steel reactor is 20 mL) and sealed, and reacted in an oven at 140° C. for more than 24 hours. After the reaction is completed, the stainless steel reactor is gradually cooled to room temperature, and the crystals generated in the stainless steel reactor are taken out to obtain colorless block crystals, which are the hybrid photoelectric induced chromic material.
[0015] The invention provides an application of an inorganic-organic hybrid photochromic material in inkless printing, electrochromic devices, photochromic decoration, optical storage, optical switch and photoelectric display.
[0016] The invention provides an application of a hybrid photochromic material prepared by a method for preparing an inorganic-organic hybrid photochromic material in inkless printing, electrochromic devices, photochromic decoration, optical storage, optical switch and photoelectric display.
[0017] When the hybrid photoelectrochromic material crystal prepared by the present invention is irradiated by ultraviolet light, the color changes from colorless to light blue in 10 seconds, and the response rate is fast.
[0018] The crystals of the hybrid photoelectrochromic material prepared by the present invention are added to a mixed solution of 0.2 mL of PMMA solution and 0.2 mL of anhydrous ethanol, and ultrasonicated for 30 minutes until the crystals are evenly dispersed in the solution. The solution is packaged into an electrochromic device (the electrochromic device comprises two pieces of ITO conductive glass, and the solution is coated between the two pieces of ITO conductive glass and dried naturally). After the electrochromic device is powered on at a certain voltage, obvious color changes occur.
[0019] The inorganic-organic hybrid photoelectrochromic material based on 2,4,6-tris(4-pyridyl)-1,3,5-triazine prepared by the present invention has fast and reversible photochromism, and the principle of photoelectrochromism of the hybrid photoelectrochromic material is mainly the charge separation within the TPT molecule and the formation of triplet diradical products. The hybrid photoelectrochromic material prepared by the present invention has good fast and reversible photochromic performance.
[0020] Compared with the prior art, the present invention has the following technical effects:
[0021] The invention adopts a solvent-thermal synthesis method, which is simple to operate and safe in process. The invention studies the changes of 2,4,6-tris(4-pyridyl)-1,3,5-triazine-based inorganic-organic hybrid materials in the photochromic process. The material changes from colorless to light blue after 10 seconds of illumination, and reaches blue visible to the naked eye after 30 seconds. Compared with the photochromic rate of existing inorganic-organic hybrid photochromic materials, the photochromic rate of the target product organic-inorganic hybrid material of the invention is greatly improved. The hybrid photochromic material is dispersed in ethanol, and the solution is evenly coated on a microporous filter membrane with a diameter of 50 mm. Under the irradiation of a 365nm ultraviolet lamp, an obvious color change occurs, from colorless to blue, and ink-free printing can be realized. The inorganic-organic hybrid photochromic material of the invention is prepared into an electrochromic device, and a voltage is applied to change color. The hybrid photoelectrically induced chromic material prepared by the present invention has broad application prospects in the fields of inkless printing, electrochromic devices, photochromic decoration, optical storage, optical switches and optoelectronic displays. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a crystal structure stacking diagram of compound 1 obtained in Example 1 of the present invention;
[0023] Figure 2 This is a photochromic picture of the compound 1 obtained in Example 1 of the present invention changing with time;
[0024] Figure 3 is the infrared spectrum of compound 1 obtained in Example 1 of the present invention before and after irradiation;
[0025] Figure 4 is the powder diffraction pattern of compound 1 obtained in Example 1 of the present invention before and after irradiation;
[0026] Figure 5 is a thermogravimetric analysis diagram of compound 1 obtained in Example 1 of the present invention;
[0027] Figure 6 is the EPR of compound 1 obtained in Example 1 of the present invention before and after irradiation;
[0028] Figure 7 The solid-state diffuse reflectance spectrum of compound 1 obtained in Example 1 of the present invention is dependent on the illumination time;
[0029] Figure 8 The ink-free printing performance of compound 1 obtained in Example 1 of the present invention;
[0030] Fig. 9 The cyclic voltammetry curve and electrochromic image of compound 1 obtained in Example 1 of the present invention are shown;
[0031] Fig.10 This is a solid diffuse reflectance spectrum diagram of compound 1 obtained in Example 1 of the present invention as the voltage changes. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0033] In order to achieve the above-mentioned object, the molecular formula of the hybrid photoelectric chromic material of the present invention is C 36 H 20 N6O 18 Zn3, monoclinic system, space group P21 / n, unit cell parameters are α=90°, β=95.60(3)°, γ=90°.
[0034] The specific process of preparing the inorganic-organic hybrid photochromic material of the present invention is as follows:
[0035] (1) 30 mg of metal source, 10 mg of TPT, 20 mg of BTC, 4 ml of H2O, 1 mL of DMA, and 1 mL of CH3OH were mixed evenly; the metal source was Zn(ClO4)2;
[0036] (2) the mixture prepared in step (1) was placed in a stainless steel high-pressure reaction vessel with a polytetrafluoroethylene reactor, and reacted in an oven at 140° C. for more than 24 hours to obtain block-shaped colorless crystals; the volume of the stainless steel reactor was 20 mL;
[0037] (3) Drying the crystals obtained in step (2) at room temperature (to remove the solution remaining on the surface of the crystals) to prepare an inorganic-organic hybrid photochromic material.
[0038] Example 1
[0039] In this example, TPT (10 mg), BTC (20 mg), zinc perchlorate (30 mg), H2O (4 mL), DMA (1 mL), and CH3OH (1 mL) were added to a stainless steel reactor lined with polytetrafluoroethylene in sequence, mixed evenly, and then sealed. The mixture was reacted in an oven at 140°C for 36 hours. After the reaction was completed, the stainless steel reactor was gradually cooled to room temperature and taken out. The crystals generated in the stainless steel reactor were removed to obtain colorless block crystals, which were the target product, recorded as compound 1, with a yield of 58.6%. Figure 1 It is a crystal structure stacking diagram of compound 1 obtained in this example.
[0040] Figure 5 is the thermogravimetric analysis diagram of compound 1, Figure 5 It can be seen that compound 1 can be stable up to 350°C, and what is released before 350°C is physically adsorbed water, indicating that compound 1 has good thermal stability.
[0041] Comparison of reaction conditions in Example 2
[0042] A comparative test was conducted by changing the single reaction conditions of Example 1 as follows:
[0043] (1) Changing the amount of CH3OH added, the yield of compound 1 is shown in Table 1:
[0044] Table 1
[0045]
[0046] (2) Changing the reaction time, the yield of compound 1 is shown in Table 2:
[0047] Table 2
[0048]
[0049] (3) Changing the reaction temperature, the yield of compound 1 is shown in Table 3:
[0050] Table 3
[0051]
[0052] Example 2: Photochromic experiment
[0053] The light source used was a 365 nm ultraviolet lamp. The bulk crystals of compound 1 prepared in Example 1 were placed under a microscope. At room temperature, after irradiation for 10 seconds, the color of the crystals changed from colorless to light blue. After irradiation for 30 seconds, the color of the crystals reached a blue color visible to the naked eye. After irradiation for 5 minutes, the color of the crystals changed to dark blue and reached saturation. For details, see Figure 2 .
[0054] Figure 3 This is the infrared spectrum of compound 1 before and after irradiation. The irradiation time is 3 minutes. Figure 3 It can be seen that the infrared spectrum of the sample after photochromism of compound 1 has similar peak positions compared with the infrared spectrum of the sample before photochromism, indicating that the structure of the crystal has not changed before and after illumination.
[0055] Figure 4 is the simulated X-ray powder diffraction pattern of compound 1, the X-ray powder diffraction pattern of the sample before photochromism, and the X-ray powder diffraction pattern of the sample after photochromism (the sample after 5 minutes of ultraviolet light irradiation), Figure 4 It can be seen that the X-ray powder diffraction pattern of the sample of compound 1 before photochromism and the X-ray powder diffraction pattern of the sample after photochromism have similar peak positions compared with the simulated X-ray powder diffraction pattern, indicating that the structure of the crystal has not changed before and after illumination.
[0056] Figure 6 is the EPR of compound 1 before and after illumination, Figure 6 It can be seen that after 5 minutes of UV light irradiation, the peak intensity of the sample at g=2.004 increased, indicating that free radicals were generated.
[0057] Figure 7 The illumination time-dependent solid-state diffuse reflectance spectrum of compound 1 was used to detect the photochromic process in the wavelength region of 365nm ultraviolet light. As the illumination time increased, the color changed from white to blue. After continuous illumination for 5 minutes, the color no longer changed.
[0058] Example 3
[0059] 10 mg of compound 1 prepared in Example 1 was added to 0.5 mL of anhydrous ethanol, and the mixture was ultrasonically treated for 30 min until compound 1 was evenly dispersed in the anhydrous ethanol. The solution was evenly coated on a microporous filter membrane with a diameter of 50 mm and dried naturally. A pattern template (a butterfly pattern template was used in this example) was covered on the membrane. Compound 1 was illuminated with a 365 nm ultraviolet lamp, and the color changed to a more obvious blue, achieving inkless printing. The illuminated sample was placed in a dark environment and returned to colorless after 12 hours (see Figure 8 ).
[0060] Example 4
[0061] 10 mg of the compound 1 prepared in Example 1 was added to a mixed solution of 0.2 mL of PMMA solution and 0.2 mL of anhydrous ethanol, and ultrasonicated for 30 min until the compound 1 was evenly dispersed in the solution. The solution was packaged into an electrochromic device (the electrochromic device comprises two pieces of ITO conductive glass, and the solution is coated between the two pieces of ITO conductive glass and dried naturally). After the electrochromic device was powered on at a certain voltage, an obvious color change occurred (see Fig. 9 ).
[0062] The embodiments described above are only preferred embodiments of the present invention and are only used to explain the present invention, not to limit the scope of implementation of the present invention. For those skilled in the art, other implementation methods can certainly be easily made by replacement or modification based on the technical contents disclosed in this specification. Therefore, all changes and improvements made to the principles and process conditions of the present invention should be included in the scope of the patent application of the present invention.
Claims
1. An inorganic-organic hybrid photoelectric chromic material, characterized in that: The chemical formula of the hybrid photoelectrochromic material is C 36 H 20 N6O 18 Zn3, the inorganic part is Zn 2+ The organic part is 2,4,6-tris(4-pyridyl)-1,3,5-triazine and trimesic acid. It is monoclinic, with space group P21 / n. The unit cell parameters are a=7.347(3)Å, b=29.365(7)Å, c=17.723(5)Å, α=90°, β=95.60(3)°, and γ=90°.
2. The method for preparing an inorganic-organic hybrid photoelectric chromic material according to claim 1, characterized in that: The following steps are involved: The metal source, 2,4,6-tris(4-pyridyl)-1,3,5-triazine, trimesic acid, water, N,N′-dimethylacetamide and methanol are uniformly mixed to obtain a mixture, and the mixture is placed in a reaction container for reaction to obtain block-shaped colorless crystals, which are hybrid photoelectrically induced color materials.
3. The method for preparing an inorganic-organic hybrid photoelectric chromic material according to claim 2, characterized in that: The metal source is zinc perchlorate.
4. The method for preparing an inorganic-organic hybrid photoelectric chromic material according to claim 2, characterized in that: The mass ratio of the metal source, 2,4,6-tris(4-pyridyl)-1,3,5-triazine and trimesic acid is (2-4):1:(1-2).
5. The method for preparing an inorganic-organic hybrid photoelectric chromic material according to claim 2, characterized in that: The volume ratio of water, N,N'-dimethylacetamide and methanol is 4:1:(0-1).
6. The method for preparing an inorganic-organic hybrid photoelectric chromic material according to claim 2, characterized in that: The reaction temperature of the mixture is 120-140° C., and the reaction time is 24-72 hours.
7. The method for preparing an inorganic-organic hybrid photoelectric chromic material according to claim 2, characterized in that: The method comprises the following steps: 30 mg of zinc perchlorate, 10 mg of 2,4,6-tris(4-pyridyl)-1,3,5-triazine, 20 mg of trimesic acid, 4 mL of water, 1 mL of N,N′-dimethylacetamide and 1 mL of methanol are uniformly mixed to obtain a mixture, and then the mixture is added into a stainless steel reactor lined with polytetrafluoroethylene and sealed, and reacted in an oven at 140°C for more than 24 hours. After the reaction is completed, the stainless steel reactor is gradually cooled to room temperature, and crystals generated in the stainless steel reactor are taken out to obtain colorless block crystals, which are hybrid photoelectrically induced color materials.
8. Application of the inorganic-organic hybrid photochromic material according to claim 1 in inkless printing, electrochromic devices, photochromic decoration, optical storage, optical switch and optoelectronic display.
9. Application of the hybrid photoelectrochromic material prepared by the method for preparing an inorganic-organic hybrid photoelectrochromic material according to any one of claims 2 to 7 in inkless printing, electrochromic devices, photochromic decoration, optical storage, optical switch and optoelectronic display.
Citation Information
Patent Citations
Electron transfer type hybrid photochromic material and preparation method thereof
CN109336913A
Method for preparing single crystal by utilizing interface reaction
CN111118595A
Photochromic Cd complex based on 2-TPT and preparation method thereof