Ionic polymer resin as well as preparation method and application thereof

By using C1 to C4 carboxylic acid as acid solution during the preparation of ionic polymer resin, the resin is dissolved and impurities avoided wrapping, the problem of metal salt residues in the prior art is solved, and low impurity residues and high transparency are achieved Effect.

CN118909165APending Publication Date: 2024-11-08JIANGSU SAILBOAT PETROCHEMICAL CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410971930.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Prior Art In the preparation of ionic polymers, the addition of inorganic acids in the acidification and demetalization step makes it difficult to clean metal salt impurities, affecting the water absorption and transparency of the product.

Method used

C1 to C4 carboxylic acids are used as acid solution to keep the ionic polymer resin dissolved without precipitation in the acidification and demetalization step, thereby avoiding metal salt impurities wrapped in polymer particles, and selecting suitable ethylene-unsaturated carboxylic acid ester copolymerization. The ratio of substances and alkalis is controlled to control the reaction conditions and achieve low metal salt impurity residues.

Benefits of technology

It effectively reduces the residual amount of metal salt impurities in the ionic polymer resin, improves water absorption and transparency, and avoids appearance problems such as white spots in the tablet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004953489450000121
    Figure BDA0004953489450000121
  • Figure BDA0004953489450000131
    Figure BDA0004953489450000131
Patent Text Reader

Abstract

The invention provides ionic polymer resin as well as a preparation method and application thereof. The ionic polymer resin is prepared from the following raw materials: an ethylene-unsaturated carboxylic ester copolymer, alkali, C1-C4 carboxylic acid and a mixed solvent, according to the method, C1-C4 carboxylic acid is selected as an acid solution, and in the acidification demetallization step, the ionic polymer resin can be kept dissolved and not separated out while metal impurity salt is generated, so that the ionic polymer resin can be effectively prevented from being separated out from a solution, the problem that metal salt impurities are easily wrapped by the separated ionic polymer resin is fundamentally solved, and the service life of the ionic polymer resin is prolonged. The obtained ionic polymer resin is low in metal salt impurity residual quantity, so that the ionic polymer resin has low water absorption and high transparency, and the appearance problems of white spots and the like are avoided during tabletting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ion polymer resins, and in particular relates to an ion polymer resin and a preparation method and application thereof. Background Art

[0002] Ionic polymers refer to a class of polymers containing metal ions. Their molecular structure is based on a copolymer of ethylene and unsaturated carboxylic acid as the main chain, on which metal ions are introduced, and ionic bonds are used as cross-links between molecules. They have excellent transparency, wear and scratch resistance, low-temperature impact toughness, and chemical resistance. They are widely used in sports equipment such as golf balls, bowling balls, sleds, and surfboards, containers for cosmetics and perfumes, food packaging (especially vacuum skin packaging), glass layers (high-rise and architectural photovoltaic glass), automotive parts, and polar exploration equipment.

[0003] At present, the main methods for preparing ionic polymers include saponification and neutralization. Among them, the saponification method is to prepare ionic polymers using ethylene-unsaturated carboxylic acid ester copolymer as the base resin, and is prepared in the form of a solution through steps such as alkali saponification, acid demetallization, purification and desalination. Compared with the neutralization method, the saponification method has the advantages of easy availability of base resin and good product uniformity. However, when using the saponification method to prepare ionic polymers, in the step of acid demetallization, it is generally necessary to add inorganic acids such as sulfuric acid and hydrochloric acid for acidification. The addition of these inorganic acids will cause the ionic polymer to precipitate, and then cause part of the generated salt to be wrapped in the precipitated polymer particles, which is difficult to be cleaned and removed, thereby affecting the water absorption and transparency of the final product.

[0004] In the prior art, the main method for achieving low metal salt impurity residue is to reduce the particle size of the precipitated polymer particles. The smaller the particle size of the polymer particles, the less metal salt impurities they contain and the easier they are to be cleaned. For example, CN114829410A discloses a method for manufacturing an ionomer resin, which includes the following steps: (1) adding a poor solvent to a solution of a crude ionomer resin containing (meth) acrylic acid units A, (meth) acrylic acid neutralization units B and ethylene units C to precipitate a granular resin with a peak particle size of 50 to 700 μm; and (2) washing the precipitated granular resin with a washing liquid, wherein the total content of the aforementioned units A and the aforementioned units B is 6 to 10 mol% based on all the monomer units constituting the aforementioned crude ionomer resin; however, when the particle size of the polymer particles is too small, filtering is difficult, so it is generally necessary to control the particle size of the precipitated polymer particles within a certain range, which leads to a high amount of metal salt impurity residues in the obtained ionic polymer.

[0005] Therefore, it is of great research value to develop an ionomer resin with low residual metal salt impurities. Summary of the invention

[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide an ion polymer resin and a preparation method and application thereof. The ion polymer resin adopts C1-C4 carboxylic acid as acid solution, so that the obtained ion polymer resin is dissolved without precipitation in the acidification demetallization step, thereby fundamentally avoiding the problem that the precipitated ion polymer resin is easy to wrap metal salt impurities, so that the finally obtained ion polymer resin has a low residual amount of metal salt impurities, and thus has the advantages of low water absorption and high transparency.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides an ionomer resin, wherein the raw materials for preparing the ionomer resin include ethylene-unsaturated carboxylic acid ester copolymer, base, C1-C4 (eg C1, C2, C3 or C4, etc.) carboxylic acid and a mixed solvent.

[0009] The present invention selects C1-C4 carboxylic acid as acid solution, and in the acid addition and acidification demetallization step, ensures that the metal impurity salt is generated while the ion polymer resin is kept dissolved without precipitation, thereby effectively preventing the generated ion polymer resin from precipitating from the solution, thereby fundamentally solving the problem that the precipitated ion polymer resin is easy to wrap the metal salt impurities, so that the residual amount of metal salt impurities in the obtained ion polymer resin is low, and thus the ion polymer resin has a lower water absorption rate and a higher transparency, and the tableting will not have appearance problems such as white spots.

[0010] Preferably, the mass percentage of ethylene-unsaturated carboxylate copolymer in the raw material for preparing the ionomer resin is 10-50%, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%.

[0011] Preferably, the mass percentage of the unsaturated carboxylate unit in the ethylene-unsaturated carboxylate copolymer is 7-35%, for example, 7%, 10%, 15%, 20%, 25%, 30% or 35%.

[0012] Preferably, the melt index of the ethylene-unsaturated carboxylate copolymer is 5 to 300 g / 10 min, for example 5 g / 10 min, 10 g / 10 min, 20 g / 10 min, 50 g / 10 min, 100 g / 10 min, 150 g / 10 min, 200 g / 10 min, 250 g / 10 min or 300 g / 10 min, the test temperature is 190° C., and the load is 2.16 kg.

[0013] Preferably, the ethylene-unsaturated carboxylic acid ester copolymer includes ethylene-butyl acrylate copolymer (EnBA) and / or ethylene-methyl methacrylate copolymer, and more preferably ethylene-butyl acrylate copolymer.

[0014] Preferably, the EnBA includes any one of EnBA2020, EnBA27150 or EnBA33150, or a combination of at least two of them.

[0015] Preferably, the molar ratio of the unsaturated carboxylate unit to the base in the ethylene-unsaturated carboxylate copolymer is 1:(1-1.5), for example, 1:1.05, 1:1.1, 1:1.15, 1:1.2, 1:1.25, 1:1.3, 1:1.35, 1:1.4, 1:1.45 or 1:1.5, etc., more preferably 1:(1-1.2), and even more preferably 1:(1.05-1.1).

[0016] Preferably, the base comprises sodium hydroxide and / or potassium hydroxide.

[0017] Preferably, the molar ratio of the base to the C1-C4 carboxylic acid is 1:(0.1-1), for example 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9 or 1:1, etc.

[0018] Preferably, the C1-C4 carboxylic acid includes any one of formic acid, acetic acid, oxalic acid, propionic acid, malonic acid, tricarballylic acid, acrylic acid, methacrylic acid, butyric acid or succinic acid, or a combination of at least two thereof, and more preferably formic acid and / or acetic acid.

[0019] Preferably, the mixed solvent includes an alcohol solvent and an aromatic solvent;

[0020] Preferably, the mass ratio of the alcohol solvent to the aromatic solvent is (1-7):(9-3), for example, 1:9, 2:8, 3:7, 4:6, 5:5, 6:4 or 7:3.

[0021] Preferably, the alcohol solvent includes any one of methanol, ethanol, tert-butanol, n-butanol or isopropanol, or a combination of at least two thereof, and methanol is more preferably used;

[0022] Preferably, the aromatic solvent includes any one of p-xylene, m-xylene, o-xylene or toluene, or a combination of at least two of them.

[0023] In a second aspect, the present invention provides a method for preparing the ionomer resin as described in the first aspect, the preparation method comprising the following steps:

[0024] (1) reacting an ethylene-unsaturated carboxylic acid ester copolymer, a base and a mixed solvent to obtain a polymer solution;

[0025] (2) Adding C1-C4 carboxylic acid to the polymer solution obtained in step (1) to carry out reaction, and obtaining the ion polymer resin through post-treatment.

[0026] Preferably, the reaction temperature in step (1) is 150-200°C, for example, 150°C, 155°C, 160°C, 165°C, 170°C, 180°C, 190°C or 200°C.

[0027] Preferably, the reaction time of step (1) is 1 to 5 h, for example, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h or 5 h.

[0028] Preferably, the method of adding the C1-C4 carboxylic acid in step (2) is any one of all-at-once addition, stepwise addition or continuous dripping, or a combination of at least two of them, more preferably stepwise addition or continuous dripping.

[0029] Preferably, the reaction temperature in step (2) is 50-100°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C.

[0030] Preferably, the reaction time of step (2) is 10 to 60 min, for example, 10 min, 20 min, 30 min, 40 min, 50 min or 60 min.

[0031] Preferably, the post-treatment method in step (2) is adding methanol to precipitate the polymer and washing with water.

[0032] Preferably, the amount of methanol added is 0.5 to 5 times the amount of the aromatic solvent added in the mixed solvent, for example, 0.5 times, 1 times, 2 times, 3 times, 4 times or 5 times.

[0033] Preferably, the temperature for adding methanol to precipitate the polymer in step (2) is 20-80°C, such as 20°C, 40°C, 60°C or 80°C.

[0034] As a preferred technical solution of the present invention, the preparation method of the ionomer resin comprises the following steps:

[0035] (1) saponification: reacting the ethylene-unsaturated carboxylic acid ester copolymer, a base and a mixed solvent at 150 to 200° C. for 1 to 5 hours to obtain a first polymer solution;

[0036] (2) Acidification: Cooling the polymer solution obtained in step (1) to 50-100° C., adding a C1-C4 carboxylic acid and reacting for 10-60 min to obtain a second polymer solution;

[0037] (3) Purification and desalting: adding methanol to the second polymer solution obtained in step (2) at 20-80° C. to precipitate the polymer, and washing and drying to obtain the ionic polymer resin.

[0038] In a third aspect, the present invention provides an application of the ionic polymer as described in the first aspect, wherein the application includes use in preparing sports equipment, cosmetic containers, perfume containers, food packaging, glass laminates, automotive parts or polar exploration equipment.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] The raw materials for preparing the ion polymer resin provided by the present invention include ethylene-unsaturated carboxylic acid ester copolymer, alkali, C1-C4 carboxylic acid and mixed solvent; by selecting C1-C4 carboxylic acid as acid solution, in the acidification and demetallization step, metal impurity salt can be generated while keeping the ion polymer resin dissolved without precipitation, thereby effectively preventing the ion polymer resin from precipitating from the solution, fundamentally solving the problem that the precipitated ion polymer resin is easy to wrap metal salt impurities, so that the residual amount of metal salt impurities in the obtained ion polymer resin is low (<200ppm), the water absorption rate is low and the transparency rate is high, and the appearance problems such as white spots will not appear in the tableting. DETAILED DESCRIPTION

[0041] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0042] Some of the raw material information involved in the following examples is as follows:

[0043] (1) Ethylene butyl acrylate (EnBA)

[0044] EnBA 20020: melt index is 20 g / 10 min, 190°C, the mass percentage of butyl acrylate structure is 20%, purchased from Repsol, brand name E20020;

[0045] EnBA 27150: melt index is 150 g / 10 min, 190°C, the mass percentage of butyl acrylate structure is 27%, purchased from Repsol, brand name E27150;

[0046] EnBA 33150: melt index is 150 g / 10 min, 190° C., the mass percentage of butyl acrylate structure is 33%, purchased from Repsol, brand number E33150.

[0047] (2) Methanol, p-xylene, sodium hydroxide (NaOH), formic acid and acetic acid: all are AR grade, Chinese medicine reagents.

[0048] Example 1

[0049] An ionomer resin, prepared from raw materials including 60 g EnBA 20020, 4.1 g NaOH, 0.6 g acetic acid, 112 g p-xylene and 28 g methanol;

[0050] The preparation method of the ionomer resin provided in this embodiment includes the following steps:

[0051] (1) Saponification: EnBA 20020, NaOH, methanol and p-xylene are placed in a container, heated to 180° C. and reacted for 1.5 hours to obtain a first polymer solution;

[0052] (2) Acidification: Cool the first polymer solution to 90° C., add acetic acid at one time and react for 1 h to obtain a second polymer solution;

[0053] (3) Purification and desalting: at 65° C., methanol was added to the second polymer solution (the amount of methanol added was 1.5 times that of p-xylene) to precipitate the polymer, which was then washed with water three times and dried to obtain the ion polymer resin.

[0054] Example 2

[0055] An ionomer resin, wherein the raw materials for preparing the resin include 60 g of EnBA 20020, 4.1 g of NaOH, 2.8 g of acetic acid, 28 g of methanol and 112 g of p-xylene;

[0056] The preparation method of the ionomer resin provided in this embodiment includes the following steps:

[0057] (1) Saponification: EnBA 20020, NaOH, methanol and p-xylene are placed in a container, heated to 180° C. and reacted for 2 hours to obtain a first polymer solution;

[0058] (2) Acidification: cool the first polymer solution to 90° C., add acetic acid at once and react for 1 h to obtain a second polymer solution;

[0059] (3) Purification and desalting: at 65° C., methanol was added to the second polymer solution (the amount of methanol added was 1.5 times that of p-xylene) to precipitate the polymer, which was then washed with water three times and dried to obtain the ion polymer resin.

[0060] Example 3

[0061] An ionomer resin, wherein the raw materials for its preparation include 60g EnBA 20020, 4.1g NaOH, 4.5g acetic acid, 28g methanol and 112g p-xylene;

[0062] The preparation method of the ionomer resin provided in this embodiment includes the following steps:

[0063] (1) Saponification: EnBA 20020, NaOH, methanol and p-xylene are placed in a container, heated to 180° C. and reacted for 4 hours to obtain a first polymer solution;

[0064] (2) Acidification: cool the first polymer solution to 90° C. and continuously add acetic acid for 30 min. After the addition is completed, react for 1 h to obtain a second polymer solution.

[0065] (3) Purification and desalting: at 65° C., methanol was added to the second polymer solution (the amount of methanol added was 1.5 times that of p-xylene) to precipitate the polymer, which was then washed with water three times and dried to obtain the ion polymer resin.

[0066] Example 4

[0067] An ionomer resin, wherein the raw materials for its preparation include 60g EnBA 20020, 4.1g NaOH, 6.2g acetic acid, 112g p-xylene and 28g methanol;

[0068] The preparation method of the ionomer resin provided in this embodiment includes the following steps:

[0069] (1) Saponification: EnBA20020, NaOH, methanol and p-xylene are placed in a container, heated to 180° C. and reacted for 1.5 hours to obtain a first polymer solution;

[0070] (2) Acidification: Cool the first polymer solution to 90° C., add acetic acid at one time and react for 0.2 h to obtain a second polymer solution;

[0071] (3) Purification and desalting: at 45° C., methanol was added to the second polymer solution (the amount of methanol added was 1 times that of p-xylene) to precipitate the polymer, which was then washed with water three times and dried to obtain the ionomer resin.

[0072] Example 5

[0073] An ionomer resin, wherein the raw materials for its preparation include 60g EnBA 20020, 4.1g NaOH, 4.5g acetic acid, 112g p-xylene and 28g methanol;

[0074] The preparation method of the ionomer resin provided in this embodiment includes the following steps:

[0075] (1) Saponification: EnBA20020, NaOH, methanol and p-xylene are placed in a container, heated to 180° C. and reacted for 2 hours to obtain a first polymer solution;

[0076] (2) Acidification: Cool the first polymer solution to 60° C., add acetic acid at one time and react for 1 hour to obtain a second polymer solution;

[0077] (3) Purification and desalting: at 65° C., methanol was added to the second polymer solution (the amount of methanol added was twice that of p-xylene) to precipitate the polymer, which was then washed with water three times and dried to obtain the ion polymer resin.

[0078] Example 6

[0079] An ionomer resin, wherein the raw materials for its preparation include 60g EnBA 20020, 5.6g NaOH, 6.1g acetic acid, 112g p-xylene and 28g methanol;

[0080] The preparation method of the ionomer resin provided in this embodiment includes the following steps:

[0081] (1) Saponification: EnBA20020, NaOH, methanol and p-xylene are placed in a container, heated to 160° C. and reacted for 2 hours to obtain a first polymer solution;

[0082] (2) Acidification: Cool the first polymer solution to 90° C., add acetic acid at one time and react for 1 h to obtain a second polymer solution;

[0083] (3) Purification and desalting: at 70° C., methanol was added to the second polymer solution (the amount of methanol added was 1.5 times that of p-xylene) to precipitate the polymer, which was then washed with water three times and dried to obtain the ion polymer resin.

[0084] Example 7

[0085] An ionomer resin, wherein the raw materials for its preparation include 60g EnBA 27150, 5.6g NaOH, 6.1g acetic acid, 56g p-xylene and 86g methanol;

[0086] The preparation method of the ionomer resin provided in this embodiment includes the following steps:

[0087] (1) Saponification: EnBA27150, NaOH, methanol and p-xylene are placed in a container, heated to 180° C. and reacted for 2 hours to obtain a first polymer solution;

[0088] (2) Acidification: Cool the first polymer solution to 90° C., add acetic acid at one time and react for 2 h to obtain a second polymer solution;

[0089] (3) Purification and desalting: at 65° C., methanol was added to the second polymer solution (the amount of methanol added was 1.5 times that of p-xylene) to precipitate the polymer, which was then washed with water three times and dried to obtain the ion polymer resin.

[0090] Example 8

[0091] An ionomer resin, wherein the raw materials for its preparation include 60g EnBA 33150, 6.8g NaOH, 7.5g acetic acid, 56g p-xylene and 86g methanol;

[0092] The preparation method of the ionomer resin provided in this embodiment includes the following steps:

[0093] (1) Saponification: EnBA33150, NaOH, methanol and p-xylene are placed in a container, heated to 180° C. and reacted for 2 hours to obtain a first polymer solution;

[0094] (2) Acidification: Cool the first polymer solution to 90° C., add acetic acid at one time and react for 1 h to obtain a second polymer solution;

[0095] (3) Purification and desalting: at 65° C., methanol was added to the second polymer solution (the amount of methanol added was 1.5 times that of p-xylene) to precipitate the polymer, which was then washed with water three times and dried to obtain the ion polymer resin.

[0096] Example 9

[0097] An ionomer resin, wherein the raw materials for its preparation include 60g EnBA 20020, 4.1g NaOH, 3.5g formic acid, 112g xylene and 28g methanol;

[0098] The preparation method of the ionomer resin provided in this embodiment includes the following steps:

[0099] (1) Saponification: EnBA 20020, NaOH, methanol and xylene are placed in a container, heated to 180° C. and reacted for 1.5 h to obtain a first polymer solution;

[0100] (2) Acidification: Cool the first polymer solution to 90° C., add formic acid at one time and react for 1 hour to obtain a second polymer solution;

[0101] (3) Purification and desalting: at 65° C., methanol was added to the second polymer solution (the amount of methanol added was 1.5 times that of p-xylene) to precipitate the polymer, which was then washed with water three times and dried to obtain the ion polymer resin.

[0102] Example 10

[0103] An ionomer resin, wherein the raw materials for its preparation include 15g EnBA 20020, 1.0g NaOH, 1.2g formic acid, 112g p-xylene and 28g methanol;

[0104] The preparation method of the ionomer resin provided in this embodiment includes the following steps:

[0105] (1) Saponification: EnBA 20020, NaOH, methanol and p-xylene are placed in a container, heated to 180° C. and reacted for 1.5 hours to obtain a first polymer solution;

[0106] (2) Acidification: Cool the first polymer solution to 70° C., add formic acid at one time and react for 1 hour to obtain a second polymer solution;

[0107] (3) Purification and desalting: at 65° C., methanol was added to the second polymer solution (the amount of methanol added was 1.5 times that of p-xylene) to precipitate the polymer, which was then washed with water three times and dried to obtain the ion polymer resin.

[0108] Embodiment 11

[0109] An ion polymer resin, which differs from Example 1 in that acetic acid is replaced by an equal molar amount of oxalic acid, and other substances, amounts and preparation methods are all the same as those of Example 1.

[0110] Example 12

[0111] An ion polymer resin, which differs from Example 1 in that acetic acid is replaced by butyric acid in an equal mole, and other substances, amounts and preparation methods are all the same as those of Example 1.

[0112] Comparative Example 1

[0113] An ion polymer resin is different from Example 1 in that 7.4 g of hydrochloric acid with a mass percentage of 37% is used to replace 0.6 g of acetic acid, and other substances, amounts and preparation methods are all the same as those of Example 1.

[0114] Comparative Example 2

[0115] An ion polymer resin is different from Example 1 in that 5.1 g of hydrochloric acid with a mass percentage of 37% is used to replace 0.6 g of acetic acid, and other substances, amounts and preparation methods are all the same as those of Example 1.

[0116] Comparative Example 3

[0117] An ion polymer resin is different from Example 1 in that 16.8 g of sulfuric acid (mass percentage: 30%) is used to replace 0.6 g of acetic acid, and other substances, dosages and preparation methods are the same as those of Example 1.

[0118] Comparative Example 4

[0119] An ionomer resin, which differs from Example 1 in that acetic acid is replaced by equimolar valeric acid, and other substances, amounts and preparation methods are the same as those of Example 1.

[0120] Performance Test:

[0121] (1) Metal residue: Anion content in ion polymer resin, such as acetate ion, chloride ion, sulfate ion, etc., was tested using an ion chromatograph (CIC-D160);

[0122] (2) White spots on tablets: The ionomer resin was pressed at 180°C and 30 MPa for 3 min to form a 2 mm thin sheet. A tablet sample was obtained and its surface was visually observed for white spots.

[0123] The ionomer resins provided in Examples 1 to 12 and Comparative Examples 1 to 4 were tested according to the above test method. The test results are shown in Table 1:

[0124] Table 1

[0125]

[0126]

[0127] From the data in Table 1, we can see that:

[0128] (1) The metal residues in the ionomer resins provided in Examples 1 to 10 were all less than 200 ppm, and no white spots appeared after tableting, indicating that the transparency was high.

[0129] (2) Compared with Example 1, Comparative Examples 1-2 used hydrochloric acid as the acid solution for acidification, resulting in the metal residue of the obtained ionomer resin being as high as 1800-20000 ppm, and a large number of white spots appeared after tableting.

[0130] (3) Compared with Example 1, Comparative Example 3 uses sulfuric acid as the acid solution for acidification, which also results in the metal residue of the obtained ionomer resin being as high as 25,000 ppm, and a large number of white spots appearing after tableting.

[0131] (4) Compared with Example 1, Comparative Example 4 used valeric acid with a C number of 5 for acidification, resulting in a metal residue in the obtained ionomer resin greater than 2000 ppm, and a large number of white spots appeared after tableting.

[0132] (5) Compared with Example 1, Examples 11-12 respectively use oxalic acid and butyric acid instead of acetic acid as the acid solution, which also results in an increase in the metal residue in the obtained ionomer resin.

[0133] The applicant declares that the present invention illustrates an ionomer resin and its preparation method and application through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An ionomer resin, It is characterized in that The raw materials for preparing the ion polymer resin include ethylene-unsaturated carboxylic acid ester copolymer, alkali, C1-C4 carboxylic acid and mixed solvent.

2. The ionomer resin according to claim 1, It is characterized in that The mass percentage of ethylene-unsaturated carboxylic acid ester copolymer in the raw material for preparing the ionomer resin is 10-50%; Preferably, the mass percentage of the unsaturated carboxylate unit in the ethylene-unsaturated carboxylate copolymer is 7 to 35%; Preferably, the melt index of the ethylene-unsaturated carboxylic acid ester copolymer is 5 to 300 g / 10 min; Preferably, the ethylene-unsaturated carboxylic acid ester copolymer includes ethylene-butyl acrylate copolymer and / or ethylene-methyl methacrylate copolymer, and more preferably ethylene-butyl acrylate copolymer.

3. The ionomer resin according to claim 1 or 2, It is characterized in that The molar ratio of the unsaturated carboxylic acid ester unit to the base in the ethylene-unsaturated carboxylic acid ester copolymer is 1:(1-1.5), preferably 1:(1-1.2), and more preferably 1:(1.05-1.1); Preferably, the base comprises sodium hydroxide and / or potassium hydroxide.

4. The ionomer resin according to any one of claims 1 to 3, It is characterized in that The molar ratio of the base to the C1-C4 carboxylic acid is 1:(0.1-1); Preferably, the C1-C4 carboxylic acid includes any one of formic acid, acetic acid, oxalic acid, propionic acid, malonic acid, tricarballylic acid, acrylic acid, methacrylic acid, butyric acid or succinic acid, or a combination of at least two thereof, and more preferably formic acid and / or acetic acid.

5. The ionomer resin according to any one of claims 1 to 4, It is characterized in that The mixed solvent includes an alcohol solvent and an aromatic solvent; Preferably, the alcohol solvent includes any one of methanol, ethanol, tert-butanol, n-butanol or isopropanol, or a combination of at least two thereof, and methanol is more preferably used; Preferably, the aromatic solvent includes any one of p-xylene, m-xylene, o-xylene or toluene, or a combination of at least two of them.

6. A method for preparing the ionomer resin according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: (1) reacting an ethylene-unsaturated carboxylic acid ester copolymer, a base and a mixed solvent to obtain a polymer solution; (2) Adding C1-C4 carboxylic acid to the polymer solution obtained in step (1) to carry out reaction, and obtaining the ion polymer resin through post-treatment.

7. The preparation method according to claim 6, It is characterized in that The reaction temperature of step (1) is 150-200° C. and the reaction time is 1-5 hours.

8. The preparation method according to claim 6 or 7, It is characterized in that The method of adding the C1-C4 carboxylic acid in step (2) includes any one of all-at-once addition, portion-wise addition or continuous dropwise addition or a combination of at least two of them, preferably portion-wise addition or continuous dropwise addition; Preferably, the reaction temperature in step (2) is 50-100° C. and the reaction time is 10-60 min.

9. The preparation method according to any one of claims 6 to 8, It is characterized in that The post-treatment method in step (2) is to add methanol to precipitate the polymer and wash with water; Preferably, the amount of methanol added is 0.5 to 5 times the amount of the aromatic solvent added in the mixed solvent; Preferably, the temperature for adding methanol to precipitate the polymer in step (2) is 20-80°C.

10. Use of the ionic polymer according to any one of claims 1 to 5, It is characterized in that The applications include the production of sports equipment, cosmetic containers, perfume containers, food packaging, glass laminations, automotive components or polar exploration equipment.