Anti-aging poly-alpha-olefin as well as preparation method and application thereof

By introducing amine groups and sterically hindered phenolic monomers with olefins to optimize polymerization conditions, the problem of aging of polyα-olefin materials under high temperature and ultraviolet light is solved, and the long-term stability and anti-aging performance of the material are improved. Broaden its scope of use in industrial applications.

CN118909172AActive Publication Date: 2024-11-08TIANJIN UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410975864.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing polyα-olefin materials have deteriorated performance when photooxygen or thermal oxygen aging, and their anti-aging performance is unstable, especially when they are easily aged under high temperature and ultraviolet light, which limits their widespread use in industrial applications.

Method used

By introducing amine-based monomers and sterically hindered phenolic monomers, the polymerization conditions are optimized, and anti-aging polyα-olefins with thermal oxygen stability and ultraviolet stability are synthesized. These functional monomers are used to copolymerize with olefins to design and synthesize a series of anti-aging Polymers avoid catalyst poisoning and functional group aggregation, and improve the dispersion and stability of the polymer.

Benefits of technology

The long-term stability of polyα-olefin materials under high temperature and ultraviolet light has been achieved, the service life has been extended, the anti-aging performance of the material has been improved, the spillover problem of small molecule additives has been avoided, and the material has been significantly improved. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909172A_ABST
    Figure CN118909172A_ABST
Patent Text Reader

Abstract

The invention provides anti-aging poly-alpha-olefin as well as a preparation method and application thereof, and belongs to the technical field of organic synthesis. The preparation method of the anti-aging poly-alpha-olefin provided by the invention comprises the following steps: mixing an amino monomer or a sterically hindered phenol monomer with a hydrocarbon compound to obtain a mixed solution, introducing an alpha-olefin compound into the mixed solution, and sequentially adding a cocatalyst and a catalyst for polymerization reaction to obtain a target product. According to the invention, the copolymerized functional monomer is introduced into poly-alpha-olefin, so that the photo-oxidative aging resistance and thermo-oxidative aging resistance of the polymer can be effectively improved, and the generation of surface cracks and the aging of materials in the process of heating or irradiating a sample and the like are remarkably inhibited. When the oxidation aging time exceeds 504 hours and the ultraviolet aging time exceeds 168 hours, the polymer is not obviously aged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of organic synthesis, and in particular to an anti-aging poly-alpha-olefin and a preparation method and application thereof. Background Art

[0002] With the in-depth promotion of new industrialization, informatization, urbanization and agricultural modernization and the continuous upgrading of residents' consumption structure, poly-α-olefins are used in many fields such as auto parts, energy, medical equipment, high-end pipes and packaging. While residents' requirements for the service life of auto parts are increasing, the requirements for heat-resistant oxygen and light-resistant oxygen aging of high-end pipes are also increasing. At present, the anti-aging performance of polyolefin materials is mainly achieved by adding small molecule anti-aging additives containing hindered phenols and hindered amines. During use, this type of antioxidant is prone to agglomeration and overflow from the non-polar polyolefin matrix, resulting in attenuation or failure of anti-aging performance, and even safety hazards. Some packaging fields involving food, medicine, etc. have higher requirements for the lower limit of small molecule dissolutions, so it is urgent to have higher stability and safety while ensuring the mechanical properties of the material itself to avoid the dissolution of small molecule additives. The market demand for anti-aging olefin polymer materials will continue to grow and the requirements will be higher. However, the synthesis of poly-α-olefin materials that take into account the requirements of high heat resistance, excellent chemical stability, and UV absorption resistance is still a challenge.

[0003] Among poly-α-olefin materials, polypropylene (PP) is a thermoplastic synthetic resin with excellent performance. It is a colorless, translucent, thermoplastic, lightweight general-purpose plastic with chemical resistance, heat resistance, electrical insulation, high-strength mechanical properties and good high-wear processing performance. By controlling the conditions of the polymerization reaction and adding appropriate comonomers, the material can be given properties such as UV resistance. Polybutene (PB) is a high molecular weight inert polymer, mainly formed by the polymerization of butene. Because PB has high crystallinity and low melting point, it gives the material good rigidity and strength, and is easy to process and shape. It is suitable for packaging materials, electronic products, automotive parts, etc. In addition, the material can be given properties such as high temperature resistance and UV resistance by controlling the conditions of the polymerization reaction and adding appropriate comonomers. Poly-4-methyl-1-pentene (PMP) is a polymer material with high readability and practicality. Its structural formula is mainly a cyclic molecule composed of five carbon atoms, one of which is linked to a methyl group. Its unique structural formula has high thermal and chemical stability and is widely used in the fields of aerospace, electronics and electrical appliances, etc. By controlling the conditions of the polymerization reaction and adding appropriate comonomers, the material can be endowed with properties such as UV resistance. Therefore, the excellent performance of PB, PP and PMP makes it highlight the emerging application prospects in many fields such as packaging, electronics and pipes. However, since these two types of polymers contain a large number of tertiary carbons on the main chain or side chain, the hydrogen on the tertiary carbon is unstable. Poly-α-olefins represented by polypropylene have poor tolerance to light and heat, and are prone to photo-oxidation or thermal-oxidation aging after absorbing energy, which greatly limits their wide application in many fields. Although the addition of small molecule antioxidants can improve the aging resistance, polyolefins themselves are non-polar and have poor compatibility with polar small molecule antioxidants. During processing and use, polar small molecules are easily aggregated and slipped, affecting the long-term and stability of anti-aging performance. In order to effectively broaden the application field of poly-α-olefins and improve their service life and performance stability, it is of great significance to develop poly-α-olefin materials with stable aging resistance.

[0004] In recent years, with the continuous innovation of synthetic catalyst technology, the design and synthesis of new structures and high-value poly-α-olefin materials have emerged. Among them, anti-aging poly-α-olefins not only retain the excellent properties of polymers, but also show high resistance to heat and oxygen aging and light aging, and have broad prospects for industrial application. Since polar functional groups easily poison and inactivate olefin coordination polymerization catalysts, it is difficult to directly copolymerize poly-α-olefins with anti-aging functional groups, which makes the direct synthesis of anti-aging poly-α-olefins extremely challenging. This type of anti-aging macromolecule can also be further added to the poly-α-olefin matrix as an anti-aging modifier, which can effectively inhibit the slippage and aggregation of polar functional groups, thereby achieving better dispersibility and stability, avoiding the overflow problem of similar small molecule antioxidants, and thus ensuring the performance stability of polyolefins and further extending their service life.

[0005] In summary, there is almost no relevant research on poly-α-olefins with excellent anti-aging properties and their application as macromolecular anti-aging additives. There is a lack of establishing the connection between structure and performance on a macro scale. Relevant olefin polymer products with excellent comprehensive properties and their applications are urgently needed to be developed. Summary of the invention

[0006] Based on the above content, the present invention provides an anti-aging poly-α-olefin and its preparation method and application. The present invention realizes the synthesis of high-performance anti-aging polymer based on olefin by introducing amine monomers with thermal oxygen stability and ultraviolet stability and optimizing polymerization conditions.

[0007] In order to achieve the above object, the present invention provides the following technical solution: an anti-aging poly-α-olefin having a structural formula shown in Formula I or Formula II:

[0008]

[0009] Among them, R is selected from

[0010] The value range of n is 1-11.

[0011] The present invention also provides a method for preparing the anti-aging poly-α-olefin, comprising the following steps:

[0012] After mixing the copolymer functional monomer with the hydrocarbon compound, a mixed solution is obtained, and then an α-olefin compound is introduced into the mixed solution, and then a co-catalyst and a catalyst are added in sequence to perform a polymerization reaction to obtain the anti-aging poly α-olefin; the copolymer functional monomer is an amino monomer or a hindered phenol monomer. The general reaction formula is as follows:

[0013]

[0014] In some embodiments, the copolymerizable functional monomers include 4-(2-propenyl)diphenylaniline, 4-(3-butenyl)diphenylaniline, 4-(4-pentenyl)diphenylaniline, 4-(5-hexenyl)diphenylaniline, 4-(6-heptenyl)diphenylaniline, 4-(7-octenyl)diphenylaniline, 3-carbazole-1-propylene, 4-carbazole-1-butene, 5-carbazole-1-pentene, 6-carbazole-1-hexene, 7-carbazole-1-pentene, 1-heptene, 8-carbazole-1-octene, 9-carbazole-1-nonene, 10-carbazole-1-decene, 11-carbazole-1-undecene, 4-(2-propenyl)-2,6-diisopropylbenzene, 4-(3-butenyl)-2,6-diisopropylphenol, 4-(4-pentenyl)-2,6-diisopropylphenol, 4-(5-hexenyl)-2,6-diisopropylphenol, 4-(6-heptenyl)-2,6-diisopropylbenzene Phenol, 4-(7-octenyl)-2,6-diisopropylphenol, 4-(8-nonenyl)-2,6-diisopropylphenol, 4-(9-decenyl)-2,6-diisopropylphenol, 4-(10-undecenyl)-2,6-diisopropylphenol, 4-(2-propenyl)-2,2,6,6-tetramethylpiperidine, 4-(3-butenyl)-2,2,6,6-tetramethylpiperidine, 4-(4-pentenyl)-2,2,6,6 -tetramethylpiperidine, 4-(5-hexenyl)-2,2,6,6-tetramethylpiperidine, 4-(6-heptenyl)-2,2,6,6-tetramethylpiperidine, 4-(7-octenyl)-2,2,6,6-tetramethylpiperidine, 4-(8-nonenyl)-2,2,6,6-tetramethylpiperidine, 4-(9-decenyl)-2,2,6,6-tetramethylpiperidine or 4-(10-undecenyl)-2,2,6,6-tetramethylpiperidine.

[0015] In some embodiments, the hydrocarbon compound includes at least one of toluene and its homologues, naphthalene and its homologues, alkanes and its homologues, and cycloalkanes and its homologues.

[0016] In some embodiments, the molar concentration of the copolymerizable functional monomer in the mixed solution is 1.0 to 0.01 mol / L.

[0017] In some embodiments, the α-olefin compound is butene or 4-methyl-1-pentene.

[0018] In some embodiments, the structural formula of the catalyst is as shown in Formula III, Formula IV, Formula V, Formula VI or Formula VII (ie, the catalyst is one of Cat.1-Cat.10):

[0019]

[0020] The co-catalyst is a boron-containing compound or an alkyl aluminum;

[0021] The molar ratio of the catalyst to the co-catalyst is 100:1 to 3000:1.

[0022] In some embodiments, the boron-containing compound includes triethylammonium tetra(phenyl)boron, tributylammonium tetra(phenyl)boron, trimethylammonium tetra(phenyl)boron, tripropylammonium (phenyl)boron, trimethylammonium tetra(p-tolyl)boron, trimethylammonium tetra(o,p-dimethylphenyl)boron, tributylammonium tetra(p-trifluoromethylphenyl)boron, trimethylammonium tetra(p-trifluoromethylphenyl)boron or tributylammonium tetra(pentafluorophenyl)boron;

[0023] The alkylaluminum includes trimethylaluminum, triethylaluminum, triisobutylaluminum, tripropylaluminum, tributylaluminum, dimethylaluminum chloride, triisopropylaluminum, tri-sec-butylaluminum, tripentylaluminum, triisopentylaluminum, tricyclopentylaluminum, trihexylaluminum, trioctylaluminum, ethyldimethylaluminum, methyldiethylaluminum, triphenylaluminum, tri-p-methylphenylaluminum, methoxyaluminum or dimethylmethoxyaluminum.

[0024] In some embodiments, the polymerization reaction is carried out at a temperature of 25 to 120° C. and for a time of 10 to 120 min.

[0025] In some embodiments, after the polymerization reaction is completed, the step of separating the product is further included; the separation step is specifically as follows: after the reaction is completed, a terminator is added to terminate the reaction, and then an acidified precipitant is added, followed by filtering, washing, and drying in sequence; the terminator is ethanol; the precipitant includes one or more of ethanol, methanol, petroleum ether, ether, n-hexane, acetone, n-pentane, tetrahydrofuran or dichloromethane.

[0026] The present invention utilizes the copolymer obtained by copolymerizing amino and hindered phenol functional monomers with olefins to have the characteristics of anti-aging performance. It is particularly noted that this characteristic can also be maintained under the condition of low functional monomer content in the copolymer. Therefore, the design and synthesis of amino monomers or hindered phenol monomers are the key to preparing a series of excellent anti-aging polymers. At the same time, by designing large sterically hindered phenolic hydroxyl monomers or amino monomers, and appropriately extending the number of carbon atoms between the olefin bond and the functional group, the catalyst poisoning phenomenon in the coordination process can be effectively avoided, the effective insertion of functional monomers in the copolymerization process is achieved, and the reduction of catalytic activity is avoided. In addition, a series of synthesized poly-alpha-olefins are characterized, and high-temperature nuclear magnetic carbon spectra are used to characterize the microscopic chemical structure of the polymer, high-temperature GPC is used to test the molecular weight and distribution of the polymer, DSC is used to study the thermal behavior of the polymer, and optical microscopy is used to observe the surface morphology of the sample.

[0027] The present invention mainly utilizes different reaction systems composed of amino monomers, hindered phenol monomers and olefin compounds, optimizes the ratio of main catalyst and co-catalyst and the reaction temperature, and synthesizes a series of poly-α-olefins that are resistant to thermal oxidation aging for 24 to 504 hours and resistant to ultraviolet aging for 24 to 168 hours. Firstly, based on the copolymerization ability of the catalyst to functionalized amino olefin monomers or hindered phenol olefin monomers with 1-olefins to a certain extent, the effects of functionalized monomer concentration, polymerization time, temperature, the ratio of different types of co-catalysts and main catalysts on polymer composition and properties, and the effect of functional group content on anti-aging properties are systematically studied, so as to achieve efficient regulation of the anti-aging properties of poly-α-olefins. 13 C NMR results show that different functional monomer initial concentrations can obtain polyα-olefins with different monomer insertion rates. Different aging degrees of the obtained copolymers were tested by different thermal oxidation aging and ultraviolet irradiation treatments. In addition, the anti-aging ability of poly1-olefin can be effectively improved by blending polyα-olefins with different degrees of anti-aging as macromolecular additives with poly1-olefins without anti-aging additives. Combined with the surface morphology and characterization results of the samples, it is shown that after the same aging treatment, the cracks on the surface of amine-functionalized polyα-olefins are significantly less than those of untreated polyα-olefins; the cracks on the surface of polyα-olefins with polyα-olefin macromolecular additives are significantly less than those of untreated commercial polyolefins, indicating that this type of functionalized polyα-olefins itself has high anti-aging properties and can be used as anti-aging agents for polyα-olefins, which can not only improve the compatibility with the matrix, but also improve its aging resistance and avoid the agglomeration and overflow of aging-resistant functional groups. In summary, the improvement of anti-aging properties plays a vital role in broadening the wide application of polyα-olefins in various fields.

[0028] The insertion rate of the amino monomer in the anti-aging poly-α-olefin provided by the present invention is 0.5-5% (or the conversion rate is 40%-90%), T m =50~240℃, the weight average molecular weight of the polymer is 5×10 3 ~50×10 4 g / mol, PDI is between 2.1 and 3.2, and activity is between 60 and 90×10 5 kg polymer ·mmol Cat. -1 ·h -1 The thermal oxidative aging time of poly-α-olefin is greater than 504h, and the UV aging time is greater than 168h. When blended with commercial polyolefin products, the thermal oxidative aging time of the blend is greater than 504h, and the UV aging time is greater than 168h.

[0029] The present invention also provides an anti-aging polymer blend material, the raw materials of which include the anti-aging poly-α-olefin and a polymer; the anti-aging poly-α-olefin accounts for 1-10 wt % in the anti-aging polymer blend material.

[0030] The present invention discloses the following technical effects:

[0031] The present invention uses different copolymerization reaction systems composed of amino functional monomers or hindered phenol type functional monomers and α-olefins to synthesize a series of poly α-olefins with anti-aging properties. According to the characteristics of efficient and adjustable functional monomer types and contents, the anti-aging properties of poly α-olefins can be efficiently controlled. The insertion rate of the polymer prepared by the present invention is adjustable between 0.5% and 5%, and the molecular weight is between 5×10 3 ~50×10 4 g / mol. The mechanical properties and anti-aging properties of poly-α-olefin can be optimized by the insertion rate. When the insertion rate reaches above 0.55%, the polymer exhibits excellent anti-aging properties. For example, when the oxidation aging time exceeds 504h and the UV aging time exceeds 168h, the polymer does not age significantly.

[0032] The poly-α-olefin provided by the present invention is used as a macromolecular auxiliary agent and blended with a commercial polymer. By adjusting the ratio, a series of anti-aging blends are obtained. The auxiliary agent content of the anti-aging blend prepared by the present invention is adjustable from 1% to 10wt%. When the auxiliary agent content reaches more than 2%, the blend exhibits excellent anti-aging performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 is the butene polymer obtained in Example 1 13 C NMR spectrum;

[0035] Figure 2 The GPC curves of the polymers obtained in Examples 1, 2, and 18 before and after 168 hours of ultraviolet irradiation, wherein (a) is untreated PB, (b) is Example 1, (c) is Example 2, and (d) is Example 18;

[0036] Figure 3 The GPC curves of the polymers obtained in Examples 1, 2, and 18 before and after 96 hours of thermal oxidative aging, wherein (a) is untreated PB, (b) is Example 1, (c) is Example 2, and (d) is Example 18;

[0037] Figure 4 The OIT curves of the polymers obtained in Examples 1-3 at different thermal oxidative aging times;

[0038] Figure 5 The FT-IR partial magnified images of the polymers obtained in Examples 10-12 at different thermal oxidative aging times, wherein (a) is untreated PMP, (b) is Example 10, (c) is Example 11, and (d) is Example 12;

[0039] Figure 6 These are SEM images of the blended samples at different UV aging times after the butene polymers obtained in Examples 13 and 15 were blended with the polymer products in the prior art. DETAILED DESCRIPTION

[0040] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0041] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0042] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0043] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0044] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0045] In the preparation process, unless otherwise specified, all operations involved are performed by professionals familiar with the technical field in an MBraun glove box or using standard Schlenk technology under the protection of inert gas such as nitrogen or argon. At the same time, the solvents involved in the present invention are all solvents that are anhydrous and oxygen-free after post-treatment. In addition, in the process of preparing the anti-aging poly-α-olefin, all operations that are sensitive to moisture and oxygen are performed by professionals familiar with the technical field in an MBraun glove box or using standard Schlenk technology under the protection of nitrogen.

[0046] All polymerizations in the examples are conducted under anhydrous and oxygen-free conditions, and the polymerization bottles, syringes, ampoules and other glassware involved in the reaction, and for weighing and transferring catalysts, co-catalysts, solutions and the like, are all treated with anhydrous and oxygen-free conditions.

[0047] The present invention has carried out relevant tests on the obtained polymer, using nuclear magnetic resonance spectroscopy ( 13 CNMR) was used to characterize the chemical structure of the polymer, differential scanning calorimetry (DSC) was used to characterize the thermal properties of the polymer, high temperature gel permeation chromatography (GPC) was used to characterize the molecular weight and molecular weight distribution of the polymer, and Fourier transform infrared spectroscopy (FT-IR) was used to characterize the signal peak of the carbonyl functional group in the polymer. 1 H and 13 C NMR was measured by Bruker-400 NMR at 120°C, TMS was used as internal standard, and the solvent was deuterated o-dichlorobenzene or deuterated 1,1,2,2-tetrachloroethane. The melting temperature (T m ) was measured by differential scanning calorimeter (Q2000 DSC), and the test conditions were, under nitrogen atmosphere, the heating / cooling rate was 10℃ / min. Gel chromatography was measured using (GPC) PL GPC-220 gel permeation chromatograph. The tester was RI-Laser, PL EasiCal PS-1 was used as the standard sample, the filling column was Plgel 10μm MIXED-BLS, 1,2,4-trichlorobenzene (TCB) was used as the solvent (0.05wt% of 2,6-di-tert-butyl-4-methylphenol (BHT) was added as an antioxidant. The test temperature was 150℃ and the flow rate was 1.0mL / min. Fourier transform infrared spectroscopy was measured using Nicolet 6700 infrared spectrometer.

[0048] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0049] Example 1

[0050] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.1 catalyst):

[0051] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.25mol / L) of 4-(7-octenyl) diphenylaniline toluene solution; then, introduce 1atm butene gas and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.1 catalyst (the molar ratio of triisobutylaluminum and Cat.1 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), and stir the reaction at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain a butene polymer for subsequent characterization.

[0052] The butene polymer obtained above was subjected to NMR ( Figure 1 ) and DSC tests. The test results show that the 4-(7-octenyl)diphenylaniline insertion rate of the butene polymer obtained by polymerization in this embodiment is 0.43%, and the copolymerization activity is 88.4×10 5 g polymer ·mol Cat. -1 ·h -1 , the weight average molecular weight is 33.3×10 4 g / mol, and PDI was 3.1, indicating that the obtained butene polymer had obvious 4-(7-octenyl)diphenylaniline insertion characteristics. The specific data are shown in Table 1.

[0053] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0054] The aging treated butene polymer was photographed to observe the surface morphology changes. The test results showed that when the thermal oxidation aging time was 336h, cracks began to appear in the butene polymer sample, indicating that the sample was aged at this time. FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. OIT ( Figure 4) The test shows that the oxidation induction period of the sample of this embodiment is significantly prolonged, and the oxidation induction curve is significantly decreased, indicating that the TPA group can effectively inhibit the aging of the sample. When the ultraviolet radiation aging time is 168h, the butene polymer shows aging cracks.

[0055] Example 2

[0056] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.1 catalyst):

[0057] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.5mol / L) of 4-(7-octenyl) diphenylaniline toluene solution; then, introduce 1atm butene gas and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.1 catalyst (the molar ratio of triisobutylaluminum and Cat.1 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), and stir the reaction at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL of ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain a butene polymer for subsequent characterization.

[0058] The obtained butene polymer was subjected to NMR and DSC tests. The test results showed that the 4-(7-octenyl)diphenylaniline insertion rate of the butene polymer obtained by polymerization in this embodiment was 1.42%, and the copolymerization activity was 84.6×10 5 g polymer ·mol Cat. -1 ·h -1 , the weight average molecular weight is 18.7×10 4 g / mol, and PDI was 2.4, indicating that the obtained butene polymer has the characteristics of high insertion rate. The specific data are shown in Table 1.

[0059] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0060] The butene polymer after the aging treatment was photographed to observe the changes in the surface morphology. The test results showed that when the thermal oxidative aging time was 504 hours, the butene polymer sample had no cracks, indicating that the sample had not aged at this time. The FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidative aging was reduced. OIT ( Figure 4 ) The test shows that the oxidation induction period of the sample of this embodiment is significantly prolonged, and the oxidation induction curve is significantly decreased, indicating that the TPA group can effectively inhibit the aging of the sample. When the ultraviolet radiation aging time is 168h, the sample of the butene polymer does not show aging cracks.

[0061] Example 3

[0062] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.1 catalyst):

[0063] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.75mol / L) of 4-(7-octenyl) diphenylaniline toluene solution; then, introduce 1atm butene gas and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.1 catalyst (the molar ratio of triisobutylaluminum and Cat.1 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), and stir the reaction at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain a butene polymer for subsequent characterization.

[0064] The obtained butene polymer was subjected to NMR and DSC tests. The test results showed that the 4-(7-octenyl)diphenylaniline insertion rate of the butene polymer obtained by polymerization in this embodiment was 2.13%, and the copolymerization activity was 77.8×10 5 g polymer ·mol Cat. -1 ·h -1 , the weight average molecular weight is 16.4×10 4 g / mol, and PDI was 2.2, indicating that the obtained butene polymer has the characteristics of high insertion rate. The specific data are shown in Table 1.

[0065] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0066] The above-mentioned aging-treated butene polymer was photographed to observe the surface morphology changes. The test results showed that when the thermal oxidation aging time was 504h, the butene polymer sample had no cracks, indicating that the sample had not aged at this time. FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. OIT ( Figure 4 ) The test shows that the oxidation induction period of the sample of this embodiment is significantly prolonged, and the oxidation induction curve is significantly decreased, indicating that the TPA group can effectively inhibit polymer aging. When the ultraviolet radiation aging time is 168h, the sample of the butene polymer does not show aging cracks.

[0067] Example 4

[0068] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.2 catalyst):

[0069] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.25mol / L) of 4-(7-octenyl) diphenylaniline toluene solution; then, add 25mmol 4-methyl-1-pentene and stir for 5min; after stabilization, add 10mL of toluene solution of triisobutylaluminum and Cat.2 catalyst (the molar ratio of triisobutylaluminum and Cat.2 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), stir and react at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL methanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain 4-methyl-1-pentene polymer for subsequent characterization.

[0070] The 4-methyl-1-pentene polymer obtained above was subjected to NMR and DSC tests. The test results showed that the 4-(7-octenyl)diphenylaniline insertion rate of the 4-methyl-1-pentene polymer obtained by polymerization in this embodiment was 3.20%, the copolymerization conversion rate was 75.3%, and the weight average molecular weight was 11.9×10 4 g / mol, and PDI was 2.4, indicating that the obtained 4-methyl-1-pentene polymer has the characteristics of high insertion rate. The specific data are shown in Table 1.

[0071] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0072] The above-mentioned aging treated 4-methyl-1-pentene polymer was photographed to observe the surface morphology changes. The test results showed that when the thermal oxidation aging time was 504h, the sample of 4-methyl-1-pentene polymer did not have cracks, indicating that the sample did not age at this time. FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. OIT test showed that the oxidation induction period of the sample of this embodiment was significantly extended, and the oxidation induction curve was significantly decreased, indicating that the TPA group can effectively inhibit sample aging. When the ultraviolet radiation aging time was 168h, the sample of 4-methyl-1-pentene polymer did not have aging crack phenomenon.

[0073] Example 5

[0074] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.2 catalyst):

[0075] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.5mol / L) of 4-(7-octenyl) diphenylaniline toluene solution; then, add 25mmol 4-methyl-1-pentene and stir for 5min; after stabilization, add 10mL of toluene solution of triisobutylaluminum and Cat.2 catalyst (the molar ratio of triisobutylaluminum and Cat.2 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), stir and react at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL petroleum ether / 37wt% hydrochloric acid (volume ratio 100:1) for sedimentation, and then filtered, washed, and vacuum dried to obtain 4-methyl-1-pentene polymer for subsequent characterization.

[0076] The 4-methyl-1-pentene polymer obtained above was subjected to NMR and DSC tests. The test results showed that the 4-(7-octenyl)diphenylaniline insertion rate of the 4-methyl-1-pentene polymer obtained by polymerization in this embodiment was 3.80%, the copolymerization conversion rate was 79.5%, and the weight average molecular weight was 10.9×10 4 g / mol, and PDI was 2.7, indicating that the obtained 4-methyl-1-pentene polymer has the characteristics of high insertion rate. The specific data are shown in Table 1.

[0077] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0078] The above-mentioned aging treated 4-methyl-1-pentene polymer was photographed to observe the surface morphology changes. The test results showed that when the thermal oxidation aging time was 504h, the sample of 4-methyl-1-pentene polymer did not have cracks, indicating that the sample did not age at this time. FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. OIT test showed that the oxidation induction period of the sample of this embodiment was significantly extended, and the oxidation induction curve was significantly decreased, indicating that the TPA group can effectively inhibit sample aging. When the ultraviolet radiation aging time was 168h, the sample of 4-methyl-1-pentene polymer did not have aging crack phenomenon.

[0079] Example 6

[0080] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.2 catalyst):

[0081] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.75mol / L) of 4-(7-octenyl) diphenylaniline toluene solution; then, add 25mmol 4-methyl-1-pentene and stir for 5min; after stabilization, add 10mL of toluene solution of triisobutylaluminum and Cat.2 catalyst (the molar ratio of triisobutylaluminum and Cat.2 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), stir and react at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain 4-methyl-1-pentene polymer for subsequent characterization.

[0082] The 4-methyl-1-pentene polymer obtained above was subjected to NMR and DSC tests. The test results showed that the 4-(7-octenyl)diphenylaniline insertion rate of the 4-methyl-1-pentene polymer obtained by polymerization in this embodiment was 4.40%, the copolymerization conversion rate was 84.1%, and the weight average molecular weight was 9.4×10 4g / mol, and PDI was 2.8, indicating that the obtained 4-methyl-1-pentene polymer has the characteristics of high insertion rate. The specific data are shown in Table 1.

[0083] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0084] The above-mentioned aging treated 4-methyl-1-pentene polymer was photographed to observe the surface morphology changes. The test results showed that when the thermal oxidation aging time was 504h, the sample of 4-methyl-1-pentene polymer did not have cracks, indicating that the sample did not age at this time. FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. OIT test showed that the oxidation induction period of the sample of this embodiment was significantly extended, and the oxidation induction curve was significantly decreased, indicating that the TPA group can effectively inhibit sample aging. When the ultraviolet radiation aging time was 168h, the sample of 4-methyl-1-pentene polymer did not have aging crack phenomenon.

[0085] Example 7

[0086] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.1 catalyst):

[0087] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.25mol / L) of 11-carbazole-1-undecene toluene solution; then, introduce 1atm butene gas and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.1 catalyst (the molar ratio of triisobutylaluminum and Cat.1 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), and stir the reaction at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain a butene polymer for subsequent characterization.

[0088] The obtained butene polymer was subjected to NMR and DSC tests. The test results showed that the insertion rate of the butene polymer obtained by polymerization in this embodiment was 0.45%, and the copolymerization activity was 65.4×10 5 g polymer ·mol Cat. -1·h -1 , the weight average molecular weight is 37.6×10 4 g / mol, and PDI was 2.7, indicating that the obtained butene polymer had obvious insertion characteristics of 11-carbazole-1-undecene. The specific data are shown in Table 1.

[0089] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0090] The above-mentioned aging treated butene polymer was photographed and the surface morphology changes were observed. The test results showed that when the thermal oxidation aging time was 504h, the butene polymer sample did not show cracks, indicating that the sample did not age at this time. FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. OIT test showed that the oxidation induction period of the sample of this embodiment was significantly extended, and the oxidation induction curve was significantly decreased, indicating that the Cz group can effectively inhibit sample aging. When the ultraviolet radiation aging time was 168h, the butene polymer sample did not show aging crack phenomenon.

[0091] Example 8

[0092] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.1 catalyst):

[0093] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.5mol / L) of 11-carbazole-1-undecene toluene solution; then, introduce 1atm butene gas and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.1 catalyst (the molar ratio of triisobutylaluminum and Cat.1 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), and stir the reaction at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain a butene polymer for subsequent characterization.

[0094] The obtained butene polymer was subjected to NMR and DSC tests. The test results showed that the insertion rate of the butene polymer obtained by polymerization in this embodiment was 1.11%, and the copolymerization activity was 63.5×10 5 g polymer ·molCat. -1 ·h -1 , the weight average molecular weight is 34.2×10 4 g / mol, and a PDI of 2.6, indicating that the obtained butene polymer has obvious high insertion characteristics of 11-carbazole-1-undecene. The specific data are shown in Table 1.

[0095] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0096] The butene polymer subjected to the above aging treatment was photographed and the surface morphology changes were observed. The test results showed that when the thermal oxidation aging time was 504h, no cracks appeared in the sample of the butene polymer, indicating that the sample did not age at this time. The FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. The OIT test showed that the oxidation induction period of the sample of this embodiment was significantly prolonged, and the oxidation induction curve was significantly decreased, indicating that the Cz group can effectively inhibit the aging of the sample. When the ultraviolet radiation aging time was 168h, the sample of the butene polymer did not show aging cracks.

[0097] Example 9

[0098] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.1 catalyst):

[0099] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.75mol / L) of 11-carbazole-1-undecene toluene solution; then, introduce 1atm butene gas and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.1 catalyst (the molar ratio of triisobutylaluminum and Cat.1 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), and stir the reaction at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain a butene polymer for subsequent characterization.

[0100] The obtained butene polymer was subjected to NMR and DSC tests. The test results showed that the insertion rate of the butene polymer obtained by polymerization in this embodiment was 1.67%, and the copolymerization activity was 60.7×105 g polymer ·mol Cat. -1 ·h -1 , the weight average molecular weight is 23.2×10 4 g / mol, and a PDI of 2.1, indicating that the obtained butene polymer has obvious high insertion characteristics of 11-carbazole-1-undecene. The specific data are shown in Table 1.

[0101] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0102] The above-mentioned aging treated butene polymer was photographed and the surface morphology changes were observed. The test results showed that when the thermal oxidation aging time was 504h, the butene polymer sample did not show cracks, indicating that the sample did not age at this time. FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. OIT test showed that the oxidation induction period of the sample of this embodiment was significantly extended, and the oxidation induction curve was significantly decreased, indicating that the Cz group can effectively inhibit sample aging. When the ultraviolet radiation aging time was 168h, the butene polymer sample did not show aging crack phenomenon.

[0103] Example 10

[0104] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.2 catalyst):

[0105] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.25mol / L) of 11-carbazole-1-undecene toluene solution; then, add 25mmol 4-methyl-1-pentene and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.2 catalyst (the molar ratio of triisobutylaluminum and Cat.2 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), and stir the reaction at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain 4-methyl-1-pentene polymer for subsequent characterization.

[0106] The 4-methyl-1-pentene polymer obtained above was subjected to NMR and DSC tests. The test results showed that the 11-carbazole-1-undecene insertion rate of the 4-methyl-1-pentene polymer obtained by polymerization in this embodiment was 0.70%, the copolymerization conversion rate was 72.7%, and the weight average molecular weight was 11.9×10 4 g / mol, and a PDI of 2.4, indicating that the obtained 4-methyl-1-pentene polymer has the insertion characteristics of 11-carbazole-1-undecene. The specific data are shown in Table 1.

[0107] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0108] The 4-methyl-1-pentene polymer treated with the above aging treatment was photographed to observe the surface morphology changes. The test results showed that when the thermal oxidation aging time was 504h, the 4-methyl-1-pentene polymer sample had no cracks, indicating that the sample had not aged at this time. FT-IR ( Figure 5 ) test shows that the carbonyl absorption peak intensity of the sample of this embodiment is significantly reduced, indicating that the degree of thermal oxidative aging is reduced. The OIT test shows that the oxidation induction period of the sample of this embodiment is significantly prolonged, and the oxidation induction curve is significantly decreased, indicating that the Cz group can effectively inhibit the aging of the sample. When the ultraviolet radiation aging time is 168h, the sample of 4-methyl-1-pentene polymer does not show aging crack phenomenon.

[0109] Embodiment 11

[0110] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.2 catalyst):

[0111] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.5mol / L) of 11-carbazole-1-undecene toluene solution; then, add 25mmol of 4-methyl-1-pentene and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.2 catalyst (the molar ratio of triisobutylaluminum and Cat.2 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), and stir the reaction at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL of ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain 4-methyl-1-pentene polymer for subsequent characterization.

[0112] The 4-methyl-1-pentene polymer obtained above was subjected to NMR and DSC tests. The test results showed that the 11-carbazole-1-undecene insertion rate of the 4-methyl-1-pentene polymer obtained by polymerization in this embodiment was 1.20%, the copolymerization conversion rate was 77.3%, and the weight average molecular weight was 10.3×10 4 g / mol, and PDI was 2.4, indicating that the obtained 4-methyl-1-pentene polymer has the characteristics of high insertion rate. The specific data are shown in Table 1.

[0113] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0114] The aging-treated 4-methyl-1-pentene polymer was photographed to observe the surface morphology changes. The test results showed that when the thermal oxidation aging time was 504h, no cracks appeared in the 4-methyl-1-pentene polymer sample, indicating that the sample was not aged at this time. FT-IR ( Figure 5 ) test shows that the carbonyl absorption peak intensity of the sample of this embodiment is significantly reduced, indicating that the degree of thermal oxidative aging is reduced. The OIT test shows that the oxidation induction period of the sample of this embodiment is significantly prolonged, and the oxidation induction curve is significantly decreased, indicating that the Cz group can effectively inhibit the aging of the sample. When the ultraviolet radiation aging time is 168, the sample of 4-methyl-1-pentene polymer does not show aging crack phenomenon.

[0115] Example 12

[0116] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.2 catalyst):

[0117] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.75mol / L) of 11-carbazole-1-undecene toluene solution; then, add 25mmol of 4-methyl-1-pentene and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.2 catalyst (the molar ratio of triisobutylaluminum and Cat.2 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), and stir the reaction at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL of ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain 4-methyl-1-pentene polymer for subsequent characterization.

[0118] The 4-methyl-1-pentene polymer obtained above was subjected to NMR and DSC tests. The test results showed that the 11-carbazole-1-undecene insertion rate of the 4-methyl-1-pentene polymer obtained by polymerization in this embodiment was 1.90%, the copolymerization conversion rate was 83.1%, and the weight average molecular weight was 7.9×10 4 g / mol, and PDI was 2.9, indicating that the obtained 4-methyl-1-pentene polymer has the characteristics of high insertion rate. The specific data are shown in Table 1.

[0119] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0120] The 4-methyl-1-pentene polymer treated with the above aging treatment was photographed to observe the surface morphology changes. The test results showed that when the thermal oxidation aging time was 504h, the 4-methyl-1-pentene polymer sample had no cracks, indicating that the sample had not aged at this time. FT-IR ( Figure 5 ) test shows that the carbonyl absorption peak intensity of the sample of this embodiment is significantly reduced, indicating that the degree of thermal oxidative aging is reduced. The OIT test shows that the oxidation induction period of the sample of this embodiment is significantly prolonged, and the oxidation induction curve is significantly decreased, indicating that the Cz group can effectively inhibit the aging of the sample. When the ultraviolet radiation aging time is 168h, the sample of 4-methyl-1-pentene polymer has no aging crack phenomenon.

[0121] Example 13

[0122] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.5 catalyst):

[0123] Using a Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 1.75mol / L) of 4-(7-octenyl) diphenylaniline toluene solution; then, introduce 1atm butene gas and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.5 catalyst (the molar ratio of triisobutylaluminum to Cat.5 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), stir and react at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is dropped into a beaker containing 300mL ethanol / 37wt% hydrochloric acid (volume ratio 100:1) for sedimentation, and then filtered, washed, and vacuum dried to obtain a butene polymer.

[0124] The obtained butene polymer was subjected to NMR and DSC tests. The test results showed that the 4-(7-octenyl)diphenylaniline insertion rate of the butene polymer obtained by polymerization in this embodiment was 1.97%, and the copolymerization activity was 73.7×10 5 g polymer ·mol Cat. -1 ·h -1 , the weight average molecular weight is 18.3×10 4 g / mol, and a PDI of 2.7, indicating that the obtained butene polymer has obvious 4-(7-octenyl)diphenylaniline insertion characteristics. The specific data are shown in Table 1.

[0125] Butene polymer and BEAULON were mixed in a mass ratio of 5:95. TM The product (purchased from Mitsui Chemicals, Japan) was blended in a mixer for 5 minutes and directly extruded into an injection molding machine to prepare anti-aging butene blend samples. The blends were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0126] The blends treated with the above aging treatment were photographed to observe the changes in surface morphology. The test results showed that when the thermal oxidation aging time was 504h, no cracks appeared on the sample, indicating that the sample had not aged at this time. FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. OIT test showed that the oxidation induction period of the sample of this embodiment was significantly prolonged, and the oxidation induction curve was significantly decreased, indicating that the TPA group can effectively inhibit the aging of the sample. When the ultraviolet radiation aging time was 168h, the sample did not show aging cracks ( Figure 6 ).

[0127] Embodiment 14

[0128] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.8 catalyst):

[0129] Using a Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.75mol / L) of 4-(7-octenyl) diphenylaniline toluene solution; then, add 25mmol of 4-methyl-1-pentene and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.8 catalyst (the molar ratio of triisobutylaluminum to Cat.8 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), stir and react at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is dropped into a beaker containing 300mL of ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain a 4-methyl-1-pentene polymer.

[0130] The 4-methyl-1-pentene polymer obtained above was subjected to NMR and DSC tests. The test results showed that the 4-(7-octenyl)diphenylaniline insertion rate of the 4-methyl-1-pentene polymer obtained by polymerization in this embodiment was 9.20%, the copolymerization conversion rate was 82.7%, and the weight average molecular weight was 9.5×10 4 g / mol, and PDI was 2.4, indicating that the obtained 4-methyl-1-pentene polymer has the characteristics of high insertion rate. The specific data are shown in Table 1.

[0131] 4-methyl-1-pentene polymer and TPXMX002 product (purchased from Mitsui Chemicals, Japan) were blended in a mixer for 5 minutes at a mass ratio of 2:98, and directly extruded into an injection molding machine to prepare 4-methyl-1-pentene blend strips. The blends were subjected to accelerated thermal oxidative aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0132] The blends treated by the above aging treatment were photographed to observe the changes in surface morphology. The test results showed that when the thermal oxidative aging time was 504h, the sample of the 4-methyl-1-pentene blend did not show cracks, indicating that the sample did not age at this time. The FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidative aging was reduced. The OIT test showed that the oxidation induction period of the sample of this embodiment was significantly extended, and the oxidation induction curve was significantly decreased, indicating that the TPA group can effectively inhibit sample aging. When the ultraviolet radiation aging time was 168h, the sample of the 4-methyl-1-pentene blend did not show aging cracking.

[0133] Embodiment 15

[0134] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.9 catalyst):

[0135] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 1.75mol / L) of 11-carbazole-1-undecene toluene solution; then, introduce 1atm butene gas and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.9 catalyst (the molar ratio of triisobutylaluminum and Cat.9 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), stir and react at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain a butene polymer.

[0136] The obtained butene polymer was subjected to NMR and DSC tests. The test results showed that the insertion rate of the butene polymer obtained by polymerization in this embodiment was 1.66%, and the copolymerization activity was 59.3×10 5 g polymer ·mol Cat. -1 ·h-1 , the weight average molecular weight is 17.7×10 4 g / mol, and a PDI of 2.5, indicating that the obtained butene polymer has obvious high insertion characteristics of 11-carbazole-1-undecene. The specific data are shown in Table 1.

[0137] Butene polymer and BEAULON were mixed in a mass ratio of 10:90. TM The product (purchased from Mitsui Chemicals, Japan) was blended in a mixer for 5 minutes and directly extruded into an injection molding machine to prepare anti-aging butene blend samples. The blends were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0138] The above-mentioned aged butene blend was photographed to observe the changes in surface morphology. The test results showed that when the thermal oxidation aging time was 504h, the butene blend sample did not show cracks, indicating that no aging occurred at this time. FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. OIT test showed that the oxidation induction period of the sample of this embodiment was significantly prolonged, and the oxidation induction curve was significantly decreased, indicating that the Cz group can effectively inhibit sample aging. When the ultraviolet radiation aging time was 168h, the butene polymer sample did not show aging crack phenomenon ( Figure 6 ).

[0139] Example 16

[0140] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.10 catalyst):

[0141] Using a Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.75mol / L) of 11-carbazole-1-undecene toluene solution; then, add 25mmol of 4-methyl-1-pentene and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.10 catalyst (the molar ratio of triisobutylaluminum and Cat.10 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), stir and react at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is dropped into a beaker containing 300mL of ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain 4-methyl-1-pentene polymer.

[0142] The 4-methyl-1-pentene polymer obtained above was subjected to NMR and DSC tests. The test results showed that the 11-carbazole-1-undecene insertion rate of the 4-methyl-1-pentene polymer obtained by polymerization in this embodiment was 8.80%, the copolymerization conversion rate was 86.8%, and the weight average molecular weight was 10.3×10 4 g / mol, and PDI was 2.9, indicating that the obtained 4-methyl-1-pentene polymer has the characteristics of high insertion rate. The specific data are shown in Table 1.

[0143] 4-methyl-1-pentene polymer and TPXMX002 product (purchased from Mitsui Chemicals, Japan) were blended in a mixer for 5 minutes at a mass ratio of 10:90, and directly extruded into an injection molding machine to prepare 4-methyl-1-pentene blend strips. The blends were subjected to accelerated thermal oxidative aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0144] The blends treated with the above-mentioned aging treatment were photographed to observe the changes in surface morphology. The test results showed that when the thermal oxidative aging time was 504h, the sample of the 4-methyl-1-pentene blend did not show cracks, indicating that the sample did not age at this time. The FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidative aging was reduced. The OIT test showed that the oxidation induction period of the sample of this embodiment was significantly extended, and the oxidation induction curve was significantly decreased, indicating that the Cz group can effectively inhibit sample aging. When the ultraviolet radiation aging time was 168h, the sample of the 4-methyl-1-pentene blend did not show aging cracking.

[0145] Embodiment 17

[0146] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.1 catalyst):

[0147] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.75mol / L) of 4-(7-octenyl)-2,6-diisopropylphenol toluene solution; then, introduce 1atm propylene gas and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.1 catalyst (the molar ratio of triisobutylaluminum and Cat.1 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), and stir the reaction at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain a propylene polymer for subsequent characterization.

[0148] The obtained propylene polymer was subjected to NMR and DSC tests. The test results showed that the insertion rate of the propylene polymer obtained by polymerization in this embodiment was 2.10%, and the copolymerization activity was 72.5×10 5 g polymer ·mol Cat. -1 ·h -1 , the weight average molecular weight is 12.3×10 4 g / mol, and PDI was 2.1, indicating that the obtained propylene polymer had obvious high insertion characteristics of 4-(7-octenyl)-2,6-diisopropylphenol. The specific data are shown in Table 1.

[0149] Propylene polymer and Prime Polypro TM The product (purchased from Mitsui Chemicals, Japan) was blended in a mixer for 5 minutes and directly extruded into an injection molding machine to prepare propylene blend strips. The blends were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0150] The above-mentioned aging-treated propylene blend was photographed to observe the changes in surface morphology. The test results showed that when the thermal oxidation aging time was 504h, the sample of the propylene blend did not show cracks, indicating that the sample did not age at this time. FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. OIT test showed that the oxidation induction period of the sample of this embodiment was significantly prolonged, and the oxidation induction curve was significantly decreased, indicating that the BHT group can effectively inhibit sample aging. When the ultraviolet radiation aging time was 168h, the sample of the propylene blend did not show aging cracks.

[0151] Embodiment 18

[0152] In this embodiment, a method for preparing an anti-aging poly-α-olefin comprises the following steps (olefin coordination copolymerization using Cat.1 catalyst):

[0153] Using the Schlenk experimental apparatus, and maintaining a vacuum degree of -101.325KPa, add 30mL of toluene solution and 2ml (concentration of 0.75mol / L) of 4-(7-octenyl)-2,2,6,6-tetramethylpiperidine toluene solution; then, introduce 1atm butene gas and stir for 5min; after stabilization, add a total of 10mL of toluene solution of triisobutylaluminum and Cat.1 catalyst (the molar ratio of triisobutylaluminum and Cat.1 catalyst is 3000:1, and the concentration of triisobutylaluminum in the toluene solution is 1.5mol / L), and stir the reaction at 600rpm for 10min; after the polymerization is completed, inject 0.1mL of ethanol to terminate the polymerization. Finally, the reacted solution is poured dropwise into a beaker containing 300mL ethanol / 37wt% hydrochloric acid (volume ratio 100:1) to settle, and then filtered, washed, and vacuum dried to obtain a butene polymer for subsequent characterization.

[0154] The obtained butene polymer was subjected to NMR and DSC tests. The test results showed that the insertion rate of the butene polymer obtained by polymerization in this embodiment was 2.60%, and the copolymerization activity was 63.7×10 5 g polymer ·mol Cat. -1 ·h -1 , the weight average molecular weight is 11.7×10 4 g / mol, and PDI was 2.7, indicating that the obtained butene polymer had obvious high insertion characteristics of 4-(7-octenyl)-2,2,6,6-tetramethylpiperidine. The specific data are shown in Table 1.

[0155] The polymers were subjected to accelerated thermal oxygen aging treatment for different times (24h, 72h, 120h, 168h, 336h, 504h) and accelerated ultraviolet aging treatment for different times (24h, 48h, 72h, 96h, 120h, 168h) for subsequent characterization.

[0156] The above-mentioned aging treated butene polymer was photographed and the surface morphology changes were observed. The test results showed that when the thermal oxidation aging time was 504h, the butene polymer sample did not show cracks, indicating that the sample did not age at this time. FT-IR test showed that the carbonyl absorption peak intensity of the sample of this embodiment was significantly reduced, indicating that the degree of thermal oxidation aging was reduced. OIT test showed that the oxidation induction period of the sample of this embodiment was significantly extended, and the oxidation induction curve was significantly decreased, indicating that the TMP group can effectively inhibit sample aging. When the ultraviolet radiation aging time was 168h, the butene polymer sample did not show aging crack phenomenon.

[0157] Table 1 Performance data of α-olefin polymers prepared in Examples 1-18 a

[0158]

[0159] Note: a: Reaction conditions: Cat. = 3-10 μmol, [B] / Hf = 100-500, temperature = 25-60°C; b: Amount of amino functional monomer added; c: High temperature GPC test; d: 13C NMR calculation; e: DSC test; f: Polymerization activity calculation; g: Copolymerization conversion rate.

[0160] From the data in Table 1, it can be seen that as the insertion rate of the amine group increases (compared with Examples 1, 2 and 3), the molecular weight distribution of the polymer gradually narrows. This may be because the addition of the comonomer inhibits the transfer of the active center to a certain extent. However, it can be seen from the relevant characterization that the introduction of the amine monomer can effectively inhibit the aging behavior. Figure 2 and Figure 3 It can be seen that the blended product also has obvious anti-aging properties.

[0161] The method for preparing an olefin polymer with excellent anti-aging performance provided by the present invention broadens the wide application of olefin polymers in multiple fields and has very important practical significance.

[0162] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An anti-aging poly-α-olefin, characterized in that: It has the structural formula shown in Formula I or Formula II: Among them, R is selected from The value range of n is 1-7.

2. A method for preparing the anti-aging poly-α-olefin according to claim 1, characterized in that: The following steps are involved: After mixing the copolymer functional monomer and the hydrocarbon compound to obtain a mixed solution, an α-olefin compound is introduced into the mixed solution, and then a co-catalyst and a catalyst are added in sequence to perform a polymerization reaction to obtain the anti-aging polyα-olefin; The copolymerizable functional monomer is an amino monomer or a hindered phenol monomer.

3. The method for preparing the anti-aging poly-α-olefin according to claim 2, characterized in that: The copolymer functional monomers include 4-(2-propenyl)diphenylaniline, 4-(3-butenyl)diphenylaniline, 4-(4-pentenyl)diphenylaniline, 4-(5-hexenyl)diphenylaniline, 4-(6-heptenyl)diphenylaniline, 4-(7-octenyl)diphenylaniline, 3-carbazole-1-propene, 4-carbazole-1-butene, 5-carbazole-1-pentene, 6-carbazole-1-hexene, 7-carbazole-1-heptene, 8-carbazole-1-octene, 9-carbazole-1-nonene, 10-carbazole-1-decene, 11-carbazole-1-undecene, 4-(2-propenyl)-2,6-diisopropylbenzene, 4-(3-butenyl)-2,6-diisopropylphenol, 4-(4-pentenyl)-2,6-diisopropylphenol, 4-(5-hexenyl)-2,6-diisopropylphenol, 4-(6-heptenyl)-2,6-diisopropylphenol, 4-( 7-octenyl)-2,6-diisopropylphenol, 4-(8-nonenyl)-2,6-diisopropylphenol, 4-(9-decenyl)-2,6-diisopropylphenol, 4-(10-undecenyl)-2,6-diisopropylphenol, 4-(2-propenyl)-2,2,6,6-tetramethylpiperidine, 4-(3-butenyl)-2,2,6,6-tetramethylpiperidine, 4-(4-pentenyl)-2,2,6,6-tetramethylpiperidine methylpiperidine, 4-(5-hexenyl)-2,2,6,6-tetramethylpiperidine, 4-(6-heptenyl)-2,2,6,6-tetramethylpiperidine, 4-(7-octenyl)-2,2,6,6-tetramethylpiperidine, 4-(8-nonenyl)-2,2,6,6-tetramethylpiperidine, 4-(9-decenyl)-2,2,6,6-tetramethylpiperidine or 4-(10-undecenyl)-2,2,6,6-tetramethylpiperidine.

4. The method for preparing the anti-aging poly-α-olefin according to claim 2, characterized in that: The hydrocarbon compound includes at least one of toluene and its homologues, naphthalene and its homologues, alkanes and its homologues, and cycloalkanes and its homologues.

5. The method for preparing the anti-aging poly-α-olefin according to claim 2, characterized in that: The molar concentration of the copolymerizable functional monomer in the mixed solution is 1.0 to 0.01 mol / L.

6. The method for preparing anti-aging poly-α-olefin according to claim 2, characterized in that: The α-olefin compound is butene or 4-methyl-1-pentene.

7. The method for preparing anti-aging poly-α-olefin according to claim 2, characterized in that: The structural formula of the catalyst is shown in Formula III, Formula IV, Formula V, Formula VI or Formula VII: Wherein, in formula III, R1=2- i Pr-Ph, t Bu or CH3, R2=H or CH3; in formula V, R3=R4=CH3 or Ph, R5=CH3 or tBu; The co-catalyst is a boron-containing compound or an alkyl aluminum; The molar ratio of the catalyst to the co-catalyst is 100:1 to 3000:

1.

8. The method for preparing anti-aging poly-α-olefin according to claim 2, characterized in that: The polymerization reaction temperature is 25-120° C. and the reaction time is 10-120 min.

9. The method for preparing anti-aging poly-α-olefin according to claim 2, characterized in that: After the polymerization reaction is completed, the step of separating the product is also included.

10. An anti-aging polymer blend material, characterized in that: The raw materials include the anti-aging poly-alpha-olefin and polymer as claimed in claim 1.

Citation Information

Patent Citations

  • Incorporation of functionalized comonomers in polyolefins

    US6166161A