Water-based covalent cross-linking type binder as well as preparation method and application thereof

Through the use of a water-based covalent crosslinking binder, the dipole-dipole interaction between the phosphate group and the silicon surface and the polymer interior of the di[2-(methacryloyloxy)ethyl]phosphate esters are utilized. Cross-linking solves the problem of electrode cracking caused by volume expansion of silicon negative electrode in lithium-ion batteries, improves the cycling and mechanical properties of the battery, simplifies the preparation process and reduces costs.

CN118909178AActive Publication Date: 2024-11-08CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411136612.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The silicon negative electrode cracks the electrode due to volume expansion in lithium-ion batteries, affecting the battery's cycling performance and range, and is complex in modification and high in cost.

Method used

Using an aqueous covalent crosslinking binder, the bonding capacity is enhanced through dipole-dipole interaction between the phosphate group and the silicon surface, and through di[2-(methacryloyloxy)ethyl]phosphate Realize internal cross-linking of polymers, alleviate the cracking of the pole sheet caused by volume expansion, and improve the circulation performance of the battery.

Benefits of technology

It significantly improves the mechanical and cycling performance of lithium-ion batteries, stabilizes the electrode structure, simplifies the preparation process, and the reaction solvent is environmentally friendly and non-toxic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909178A_ABST
    Figure CN118909178A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of lithium ion battery materials, and provides a water-based covalent cross-linking type binder as well as a preparation method and application thereof. The specific preparation method of the water-based covalent cross-linking type binder comprises the following steps: dissolving a monomer A containing double bonds in deionized water, then adding di [2-(methacryloyloxy) ethyl] phosphate as a cross-linking agent, and adding an initiator to carry out polymerization reaction, thereby obtaining the water-based covalent cross-linking type binder. According to the method, construction of a three-dimensional network structure is achieved in a dynamic and static crosslinking combined mode, a phosphate group is introduced to serve as a silicon negative electrode aqueous binder component, interaction between the phosphate group and silicon is higher, the binding capacity and mechanical performance of the material are improved, in addition, the post-treatment step of a polymer is omitted in the method for preparing the pole piece in situ, and the cost is reduced. The operation is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery materials and relates to an aqueous covalent cross-linking binder and a preparation method and application thereof. Background Art

[0002] In order to solve the range problem and further reduce costs, it is imperative to develop high-energy-density lithium-ion batteries.

[0003] Silicon has become the preferred negative electrode material for the development of high energy density batteries due to its large theoretical specific capacity and abundant reserves. Silicon forms an alloy with lithium ions to store and release lithium ions. Its theoretical specific capacity is as high as 4200mAh g -1 , which is about the current commercial graphite anode (372mAh g -1 ) more than ten times. However, in actual application, due to the influence of the lithium storage form of silicon negative electrode, after forming an alloy with lithium, silicon will inevitably expand by nearly 400%. The charging and discharging process of lithium-ion batteries causes lithium ions to be repeatedly embedded and de-embedded from the silicon negative electrode. The multiple volume expansion and contraction causes stress changes inside the electrode, leading to electrode cracking, and then the electrode material pulverizes and falls off. This phenomenon will cause the battery capacity to decay sharply and affect the battery's cycle performance.

[0004] In response to the above problems, taking into account the complexity and high cost of silicon particle modification, from the perspective of aqueous covalent cross-linking binders, designing and developing a new type of aqueous covalent cross-linking binder to alleviate the volume expansion of silicon and stabilize the electrode structure has become an important topic in the related field. Summary of the invention

[0005] In view of the above problems, the present invention provides an aqueous covalently cross-linked binder and a preparation method and application thereof, wherein the phosphate groups in the binder structure can form dipole-dipole and ion-dipole interactions with the hydroxyl groups on the silicon surface, thereby improving the material's bonding ability to silicon and stabilizing the electrode structure; and the internal cross-linking of the polymer achieved by di[2-(methacryloyloxy)ethyl]phosphate can significantly improve the mechanical properties of the material, which is beneficial to alleviate the cracking of the pole piece caused by the volume expansion of the silicon negative electrode and improve the cycle performance of the battery.

[0006] The present invention provides a method for preparing a water-based covalent cross-linking binder, comprising the following steps:

[0007] The monomer A containing double bonds is dissolved in deionized water, and then di[2-(methacryloyloxy)ethyl]phosphate is added as a crosslinking agent, and an initiator is added to carry out polymerization reaction, so as to prepare a water-based covalent crosslinking adhesive.

[0008] Further, the concentration of the aqueous solution of monomer A is 0.01-0.10 g / mL, di[2-(methacryloyloxy)ethyl]phosphate accounts for 2-10 mol% of monomer A, and the initiator accounts for 1-5% of the total mass of monomer A and di[2-(methacryloyloxy)ethyl]phosphate;

[0009] Furthermore, the monomer A is one of acrylic acid, acrylamide and acrylic ester.

[0010] Furthermore, the polymerization reaction is ultraviolet light initiated polymerization.

[0011] Furthermore, the initiator used in the ultraviolet light-induced polymerization reaction is one of 754 photoinitiator, 819 photoinitiator, 1-hydroxycyclohexyl phenyl ketone and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

[0012] Furthermore, the ultraviolet light-induced polymerization is carried out for 5 to 30 minutes at a temperature of 50 to 70°C.

[0013] The water-based graft cross-linking adhesive prepared by the above preparation method.

[0014] Application of the above aqueous graft cross-linking binder in the preparation of negative electrode materials for lithium-ion batteries.

[0015] A method for preparing a negative electrode material for a lithium ion battery comprises the following steps:

[0016] Weigh a certain amount of silicon powder and conductive additives and add them to the aqueous solution of the above-mentioned water-based graft cross-linking binder, stir them evenly, then apply them on copper foil and dry them to obtain a pole piece for use;

[0017] The silicon powder has a particle size of 60 to 100 nm; the conductive additive is one or more of acetylene black, Ketjen black, Super P, and carbon nanotubes; the mass ratio of the silicon powder, the conductive additive, and the water-based graft cross-linking binder is 50 to 70:30 to 20:20 to 10;

[0018] The stirring time is 6 to 12 hours, the drying temperature is 60 to 120° C., and the drying time is 10 to 15 hours.

[0019] The lithium ion battery silicon negative electrode material is prepared by the method for preparing the lithium ion battery negative electrode material.

[0020] The beneficial effects brought by the technical solution provided by the present invention are:

[0021] 1. The present invention uses di[2-(methacryloyloxy)ethyl]phosphate as a cross-linking agent, and realizes internal cross-linking of the polymer by combining dynamic and static cross-linking to realize the construction of a covalent cross-linking network of the binder, which can significantly improve the mechanical properties of the material, help alleviate the cracking of the pole piece caused by the volume expansion of the silicon negative electrode, and improve the cycle performance of the battery; the phosphate group in its structure can form dipole-dipole and ion-dipole interactions with the hydroxyl groups on the silicon surface, thereby improving the bonding ability of the aqueous covalent cross-linking binder to silicon, stabilizing the electrode structure, and facilitating the improvement of the cycle performance.

[0022] 2. The preparation method of the aqueous covalent cross-linking binder provided by the present invention has simple synthesis conditions and the reaction solvent is environmentally friendly and non-toxic.

[0023] 3. The ultraviolet-induced polymerization method used in the preparation method of the aqueous covalent cross-linking adhesive provided by the present invention has the advantages of being simple and efficient.

[0024] 4. The present invention adopts an in-situ method for preparing the electrode, which eliminates the post-processing step of the polymer and is simple and convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The peeling performance comparison of the water-based covalent cross-linking adhesive obtained in Examples 1 and 2 and Comparative Example 1 is shown;

[0026] Figure 2 The cyclic voltammetry curve of the secondary lithium battery prepared by using the aqueous covalent cross-linking binder obtained in Example 1 at a scan rate of 0.05 mV;

[0027] Figure 3 The AC impedance spectra of the corresponding secondary lithium batteries prepared with the aqueous covalent cross-linking binders obtained in Example 1 and Comparative Example 1 after cycling;

[0028] Figure 4 The battery cycle performance diagram of the lithium battery prepared with the aqueous covalent cross-linking binder obtained in Example 1 and Comparative Examples 1 and 2 at a current density of 0.5C. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0030] It should be noted that the experimental methods described in the following embodiments are conventional methods unless otherwise specified, and the reagents and materials can be obtained from commercial channels unless otherwise specified.

[0031] The present invention provides a method for preparing a water-based covalently cross-linked polymer binder containing a phosphonic acid group, comprising the following steps:

[0032] The monomer A containing double bonds is dissolved in deionized water, and then di[2-(methacryloyloxy)ethyl]phosphate is added as a crosslinking agent, and an initiator is added to carry out polymerization reaction, so as to prepare a water-based covalent crosslinking adhesive.

[0033] In the present invention, the initiator used in the ultraviolet polymerization reaction process is one of 754 photoinitiator, 819 photoinitiator, 1-hydroxycyclohexyl phenyl ketone and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, preferably 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

[0034] In the present invention, the monomer A comprises one of acrylic acid, acrylamide and acrylates, preferably any one of acrylic acid and acrylamide; the concentration of monomer A is 0.01-0.10 g / mL, preferably 0.01-0.05 g / mL, and more preferably 0.02 g / mL.

[0035] In the present invention, di[2-(methacryloyloxy)ethyl]phosphate accounts for 1 to 10 mol%, preferably 1 to 5 mol%, and more preferably 3 mol% of monomer A; the initiator accounts for 1 to 5% of the total mass of monomer A and di[2-(methacryloyloxy)ethyl]phosphate, preferably 2 to 4%, and more preferably 2%.

[0036] In the present invention, the ultraviolet light-induced polymerization time is 5 to 30 minutes, preferably 10 to 20 minutes, and more preferably 15 minutes; the polymerization temperature is 50 to 70°C, and preferably 60°C.

[0037] The present invention provides a method for preparing the above-mentioned water-based graft cross-linking binder corresponding to the silicon negative electrode, comprising the following steps:

[0038] A certain mass of silicon powder and conductive additives are weighed into a water-based graft cross-linking binder aqueous solution, stirred evenly, and then coated on a copper foil and dried to obtain a pole piece for use.

[0039] In the present invention, the silicon powder particle size is 60-100nm, more preferably 80nm; the mass ratio of the silicon powder, conductive additive and aqueous graft cross-linking binder is 50-70:30-20:20-10, preferably 60-70:20:20-10, more preferably 60:20:20.

[0040] In the present invention, the stirring time is 6 to 12 hours, preferably 7 to 10 hours, and more preferably 8 to 9 hours; the drying temperature is 60 to 120° C., preferably 70 to 110° C., and more preferably 80 to 100° C.; and the drying time is 10 to 15 hours, and preferably 12 hours.

[0041] Example 1

[0042] Take 0.1600g of acrylic acid and dissolve it in 8mL of deionized water. After it is fully dissolved, continue to add 0.0215g of di[2-(methacryloyloxy)ethyl]phosphate, wherein the molar ratio of acrylic acid monomer to di[2-(methacryloyloxy)ethyl]phosphate is 100:3, and then add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone accounting for 2% of the total mass of acrylic acid monomer and di[2-(methacryloyloxy)ethyl]phosphate. Then, place the reaction system under ultraviolet light to initiate polymerization for 15min, and the polymerization temperature is 60°C, and finally obtain a water-based covalent cross-linking adhesive solution for standby use.

[0043] The lithium-ion battery preparation method corresponding to this case is as follows:

[0044] Take 0.1200g of silicon powder and 0.0400g of Super P in an aqueous solution containing 0.0400g of an aqueous covalent cross-linking binder, stir thoroughly for 8h to obtain a uniformly dispersed slurry, then use a coating machine to evenly coat the slurry on the surface of a 9μm copper foil, dry at 100°C for 12h, and finally cut into circular electrode sheets with a radius of 7.5mm for use.

[0045] Example 2

[0046] Take 0.1600g of acrylamide and dissolve it in 8mL of deionized water. After it is fully dissolved, continue to add 0.0219g of di[2-(methacryloyloxy)ethyl]phosphate, wherein the molar ratio of acrylamide monomer to di[2-(methacryloyloxy)ethyl]phosphate is 100:3, and then add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone accounting for 2% of the total mass of acrylamide monomer and di[2-(methacryloyloxy)ethyl]phosphate. Then, place the reaction system under ultraviolet light to initiate polymerization for 15min, and the polymerization temperature is 60°C, and finally obtain a water-based covalent cross-linking adhesive solution for standby use.

[0047] The lithium-ion battery preparation method corresponding to this case is as follows:

[0048] Take 0.1200g of silicon powder and 0.0400g of Super P in an aqueous solution containing 0.0400g of the above-mentioned aqueous covalent cross-linking binder, stir thoroughly for 8h to obtain a uniformly dispersed slurry, then use a coating machine to evenly coat the slurry on the surface of 9μm copper foil, dry at 100℃ for 12h, and finally cut into circular electrode sheets with a radius of 7.5mm for use.

[0049] Example 3

[0050] Take 0.1600g of acrylic acid and dissolve it in 8mL of deionized water. After it is fully dissolved, continue to add 0.0215g of di[2-(methacryloyloxy)ethyl]phosphate, wherein the molar ratio of acrylic acid monomer to di[2-(methacryloyloxy)ethyl]phosphate is 100:3, and then add 1-hydroxycyclohexyl phenyl ketone accounting for 3% of the total mass of acrylic acid monomer and di[2-(methacryloyloxy)ethyl]phosphate. Then, place the reaction system under ultraviolet light to initiate polymerization for 15min, and the polymerization temperature is 60°C, and finally obtain a water-based covalent cross-linking adhesive solution for standby use.

[0051] The lithium-ion battery preparation method corresponding to this case is as follows:

[0052] Take 0.1200g of silicon powder and 0.0400g of Super P in an aqueous solution containing 0.0400g of the above-mentioned water-based grafted cross-linking binder, stir thoroughly for 8h to obtain a uniformly dispersed slurry, then use a coating machine to evenly coat the slurry on the surface of 9μm copper foil, dry at 100℃ for 12h, and finally cut into circular electrode sheets with a radius of 7.5mm for use.

[0053] Comparative Example 1

[0054] Take 0.4000g of acrylic acid and dissolve it in 20mL of deionized water. After it is fully mixed, add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone initiator of 2% of the total mass of acrylic acid and stir to dissolve. Then, place the reaction system under ultraviolet light for initiation polymerization for 15 minutes at a polymerization temperature of 60°C to obtain a polyacrylic acid binder aqueous solution for use.

[0055] The lithium-ion battery preparation method corresponding to this case is as follows:

[0056] Take 0.1200g silicon powder and 0.0400g Super P in an aqueous solution containing 0.0400g of the above polymer, stir thoroughly for 8h to obtain a uniformly dispersed slurry, then use a coating machine to evenly coat the slurry on the surface of 9μm copper foil, dry at 100℃ for 12h, and finally cut into circular electrode sheets with a radius of 7.5mm for use.

[0057] Comparative Example 2

[0058] Take 0.4000 g of sodium carboxymethyl cellulose and dissolve it in 20 mL of deionized water for later use.

[0059] The lithium-ion battery preparation method corresponding to this case is as follows:

[0060] Take 0.1200g silicon powder and 0.0400g Super P in an aqueous solution containing 0.0400g of the above polymer, stir thoroughly for 8h to obtain a uniformly dispersed slurry, then use a coating machine to evenly coat the slurry on the surface of 9μm copper foil, dry at 100℃ for 12h, and finally cut into circular electrode sheets with a radius of 7.5mm for use.

[0061] Comparative Example 3

[0062] Take 0.1600g of acrylic acid and dissolve it in 8mL of deionized water. After it is fully dissolved, continue to add 0.0072g of di[2-(methacryloyloxy)ethyl]phosphate, wherein the molar ratio of acrylic acid monomer to di[2-(methacryloyloxy)ethyl]phosphate is 100:1, and then add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone accounting for 2% of the total mass of acrylic acid monomer and di[2-(methacryloyloxy)ethyl]phosphate. Then, place the reaction system under ultraviolet light to initiate polymerization for 15min, and the polymerization temperature is 60°C, and finally obtain a water-based covalent cross-linking adhesive solution for standby use.

[0063] The lithium-ion battery preparation method corresponding to this case is as follows:

[0064] Take 0.1200g of silicon powder and 0.0400g of Super P in an aqueous solution containing 0.0400g of the above-mentioned aqueous covalent cross-linking binder, stir thoroughly for 8h to obtain a uniformly dispersed slurry, then use a coating machine to evenly coat the slurry on the surface of 9μm copper foil, dry at 100℃ for 12h, and finally cut into circular electrode sheets with a radius of 7.5mm for use.

[0065] Figure 1 The peeling performance of the water-based graft cross-linking adhesive used in Example 1 and Comparative Examples 1 and 3 is compared. Figure 1 It can be seen that the peel strength of Example 1 is greatly improved compared with that of Control Example 3 and Control Example 1. This is due to the fact that the introduction of an appropriate amount of cross-linking agent promotes the interaction between the adhesive chain segments, and the network structure constructed by the dynamic and static cross-linking method enhances the bonding ability of the water-based covalent cross-linking adhesive.

[0066] Figure 2 The cyclic voltammetry curve of the secondary lithium battery prepared in Example 1 at a scan rate of 0.05 mV is shown in FIG. Figure 2 It can be seen that during multiple scans, lithium ion embedding / de-embedding peaks in silicon materials appeared at 0.01V, 0.19V, 0.37V, and 0.53V, respectively, indicating that the aqueous covalently cross-linked binder material of Example 1 did not affect the lithium ion embedding and de-embedding process in the battery and could stably exist in the electrochemical window of 0.01-1.5V;

[0067] Figure 3 The AC impedance spectra of the secondary lithium battery after cycling corresponding to Example 1 and Comparative Example 1 are shown in FIG. Figure 3 It can be seen that the SEI impedance value of the battery corresponding to Example 1 after cycling is smaller, indicating that a thin and stable solid electrolyte layer is formed in the battery, which helps to improve the transmission capacity of lithium ions, and the corresponding aqueous covalent cross-linking binder helps to maintain the stability of the internal structure of the battery;

[0068] Figure 4 The results of the lithium batteries prepared in Example 1 and Comparative Examples 1 and 2 cycled at a current density of 2.1 A / g are compared. Figure 4 It can be seen that the battery corresponding to Example 1 still has a discharge specific capacity of 1909 mAh / g after 100 cycles, and exhibits excellent cycle performance compared with the two control examples.

[0069] In the absence of conflict, the above embodiments and features in the embodiments may be combined with each other.

[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a water-based covalent cross-linking binder, characterized in that: The following steps are involved: The monomer A containing double bonds is dissolved in deionized water, and then di[2-(methacryloyloxy)ethyl]phosphate is added as a crosslinking agent, and an initiator is added to carry out polymerization reaction, so as to prepare a water-based covalent crosslinking adhesive.

2. The method for preparing a water-based covalent cross-linking binder according to claim 1, characterized in that: The concentration of the aqueous solution of monomer A is 0.01-0.10 g / mL, di[2-(methacryloyloxy)ethyl]phosphate accounts for 2-10 mol% of monomer A, and the initiator accounts for 1-5% of the total mass of monomer A and di[2-(methacryloyloxy)ethyl]phosphate.

3. The method for preparing a water-based covalent cross-linking binder according to claim 1, characterized in that: The monomer A is one of acrylic acid, acrylic esters and acrylamide.

4. The method for preparing a water-based covalent cross-linking binder according to claim 1, characterized in that: The polymerization reaction is a polymerization reaction initiated by ultraviolet light.

5. The method for preparing a water-based covalent cross-linking binder according to claim 4, characterized in that: The initiator used in the ultraviolet light initiated polymerization reaction is one of 754 photoinitiator, 819 photoinitiator, 1-hydroxycyclohexyl phenyl ketone and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

6. The method for preparing a water-based covalent cross-linking binder according to claim 4, characterized in that: The ultraviolet light initiated polymerization lasts for 5 to 30 minutes at a temperature of 50 to 70°C.

7. A water-based covalent cross-linking adhesive prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the aqueous covalent cross-linking binder as claimed in claim 7 in preparing negative electrode materials for lithium-ion batteries.

9. A method for preparing a negative electrode material for a lithium ion battery, characterized in that: The following steps are involved: Weigh a certain amount of silicon powder and conductive additives and add them to the aqueous covalent cross-linking binder solution as claimed in claim 7, stir them evenly and then apply them on copper foil and dry them to obtain a pole piece for use; The silicon powder has a particle size of 60 to 100 nm; the conductive additive is one or more of acetylene black, Ketjen black, Super P, and carbon nanotubes; the mass ratio of the silicon powder, the conductive additive, and the aqueous covalent cross-linking binder is 50 to 70:30 to 20:20 to 10; The stirring time is 6 to 12 hours, the drying temperature is 60 to 120° C., and the drying time is 10 to 15 hours.

10. A lithium ion battery silicon negative electrode material prepared by the method for preparing a lithium ion battery negative electrode material according to claim 9.

Citation Information

Patent Citations

  • Binder for secondary battery providing excellent adhesion strength and cycle property

    CN102725890A

  • Aqueous ternary positive electrode slurry and preparation method thereof

    CN111129457A

  • Lithium-sulfur battery positive electrode material, lithium-sulfur battery positive electrode plate and lithium-sulfur battery

    CN115036508A

  • Binder for carbon-coated aluminum foil and preparation method thereof

    CN116285785A

  • Grafting type water-based grafting cross-linking type binder as well as preparation method and application of grafting type water-based grafting cross-linking type binder

    CN118388717A