Main / side chain degradable acrylate polymer containing thioester and dynamic borate structure and preparation method thereof

By introducing sulfhydryl ester and dynamic borate ester structures into the acrylate polymer, the problem of insufficient mechanical properties and degradation properties in the prior art is solved, and the excellent mechanical properties and degradability properties of the material are achieved, which is suitable for high-quality materials. Recycling and recycling of value-added industries.

CN118909180AActive Publication Date: 2024-11-08SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
CN202411119046.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The existing degradable acrylate polymers have shortcomings in mechanical properties and degradation properties, and it is difficult to take into account excellent mechanical properties and environmentally friendly degradation properties, resulting in serious plastic pollution problems.

Method used

The main/side chain degradable acrylate polymer with thioester and dynamic borate structure is adopted to impart excellent mechanical properties to the material under specific conditions by crosslinking the thioester monomer and dynamic borate structure. Mild degradation.

Benefits of technology

It achieves the best mechanical properties and degradable properties of the material. It has mild degradation conditions, low energy consumption and low pollution, and is suitable for recycling and recycling of high-value-added industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004994489060000021
    Figure BDA0004994489060000021
  • Figure BDA0004994489060000022
    Figure BDA0004994489060000022
  • Figure BDA0004994489060000031
    Figure BDA0004994489060000031
Patent Text Reader

Abstract

The invention discloses a main / side chain degradable acrylate polymer containing thioester and a dynamic borate structure and a preparation method of the main / side chain degradable acrylate polymer. The preparation method comprises the following steps: firstly, synthesizing a thioester monomer containing a fragile bond, then adding a vinyl monomer containing an epoxy functional group and a polymerization inhibitor into a sulfuric acid aqueous solution, and stirring to react; adding sodium chloride after neutralization, extracting a mixture, performing reduced pressure distillation, dissolving a product in an organic solvent, adding a boric acid monomer and anhydrous magnesium sulfate, reacting, and purifying; and polymerizing the thioester monomer, the vinyl crosslinking monomer containing the dynamic borate structure and the acrylate monomer to obtain a target product. The main / side chain degradable acrylate polymer can be sensitive to ammonia, alkali and oxidation conditions through a thioester unit and a dynamic boric acid ester structure, degradation of the polymer can be achieved under mild conditions, and meanwhile dynamic crosslinking can enable the polymer to have excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to degradable acrylate, in particular to a main / side chain degradable acrylate polymer containing thioester and dynamic borate structure and a preparation method thereof. Background Art

[0002] Traditional acrylate polymers have excellent mechanical properties and chemical stability, but due to their structural stability, they are difficult to degrade in the environment, leading to serious plastic pollution problems. Therefore, the development of degradable acrylate polymers has become a research hotspot.

[0003] Main chain degradable acrylate polymers are a type of polymer that introduces degradable chemical structures or functional groups into the main chain, allowing it to degrade into small molecules under specific conditions, thereby achieving the degradation performance of the polymer and addressing environmental pollution issues.

[0004] Chinese invention patent application CN117304846A discloses a partially degradable water-based acrylic pressure-sensitive adhesive and an environmentally friendly and recyclable sealing tape; the raw material components of the acrylic pressure-sensitive adhesive include acrylic acid, methacrylic acid, acrylamide, 2-hydroxyethyl acrylate, butyl acrylate, emulsifier, initiator, deionized water, sodium hydroxide, n-dodecyl mercaptan, and water-based rosin resin. The sealing tape of this technology is obtained by coating a partially degradable water-based acrylic pressure-sensitive adhesive that dissolves in water after drying on a completely degradable hydrophilic transparent ionic cellulose film. The acrylic pressure-sensitive adhesive can be dissolved after drying and touching water, but the characteristics of this invention limit the application of the tape, and it is not suitable for many scenes such as open-air operations and transportation of goods.

[0005] Chinese invention patent CN106317346B discloses a method for preparing a degradable antifouling resin and its use, including: using lactic acid, polyols and / or polyester polyols as raw materials to synthesize a degradable polylactic acid block polymer P1; then using P1, triethylamine, methacryloyl chloride, etc. as raw materials to synthesize a polylactic acid block polymer P2; finally using P2, methacrylate monomers, etc. as raw materials to synthesize a degradable acrylate polymer P3. The degradable antifouling resin P3 prepared by this technology can be applied to degradable antifouling coatings, and the prepared antifouling coatings have excellent resistance to seawater immersion and controllable degradation. However, its tensile strength is affected by the lactic acid monomer unit: the lactic acid part will make the polymer have relatively low tensile strength and low elongation, and the lactic acid group is easy to cause brittle fracture, showing relative brittleness and low fracture toughness. Therefore, the mechanical properties of the degradable resin need to be improved.

[0006] Chinese invention patent CN115477741B discloses a degradable polymer and its preparation method and application. This technology uses ε-caprolactone monomer and hydroxyphenylboronic acid as raw materials for bulk polymerization, uses hydroxyphenylboronic acid as an initiator and catalyst, and directly obtains a degradable polymer with phenylboronic acid at the α-end and hydroxyl at the ω-end. This technology is to connect the hydroxyphenylboronic acid structure and the hydroxyl structure at both ends of the polyester-based main chain respectively. Although it can improve the water solubility of the degradable polymer composed of the polyester-based main chain, the fracture toughness and mechanical strength of the main chain degradable polymer will be very low, and it is difficult to have a high modulus, and the mechanical properties of the degradable resin are still insufficient. Summary of the invention

[0007] The object of the present invention is to provide a main / side chain degradable acrylate polymer containing a thioester and a dynamic borate structure which has both excellent mechanical properties and degradation properties and a preparation method thereof, thereby reducing resource waste and environmental pollution.

[0008] The purpose of the present invention can be achieved through the following technical solutions:

[0009] The main / side chain degradable acrylate polymer containing thioester and dynamic borate structure has the following structural formula:

[0010]

[0011] Wherein m1, m2, m3, m4 = 30-36, n1, n2, n3, n4 = 24-29;

[0012] R1 is one of the following groups:

[0013]

[0014] R2 is one of the following groups:

[0015]

[0016] R3 is one of the following groups:

[0017]

[0018] The method for preparing the main / side chain degradable acrylate polymer containing thioester and dynamic borate structure comprises the following steps:

[0019] 1) dissolving the lactone monomer in an organic solvent free of water, adding a vulcanizing agent, stirring and reacting for 5-8 hours under an inert atmosphere, removing the organic solvent, and separating by chromatography to obtain a thioester monomer;

[0020] 2) adding a vinyl monomer containing an epoxy functional group and a polymerization inhibitor to a sulfuric acid aqueous solution, stirring the obtained mixture at 70-80° C. for 2-4 hours, and cooling to room temperature; adding sodium chloride after neutralization, extracting the mixture, and distilling under reduced pressure to obtain a vinyl monomer containing a vicinal diol structure; dissolving the obtained product in an organic solvent, adding a boric acid monomer and anhydrous magnesium sulfate, stirring and reacting at room temperature for 12-24 hours, then heating to 40-60° C. and distilling under reduced pressure to remove the organic solvent described in this step, and purifying to obtain a vinyl cross-linking monomer containing a dynamic borate ester structure;

[0021] 3) After mixing deionized water, an initiator and an emulsifier, the air is replaced under an inert atmosphere; after adding a thioester monomer, a vinyl crosslinking monomer containing a dynamic borate structure and an acrylate monomer, the mixture is ultrasonically dispersed, and the mixture is stirred and reacted at 70-80° C. to obtain a main / side chain degradable acrylate polymer containing a thioester and a dynamic borate structure.

[0022] To further achieve the purpose of the present invention, preferably, in step 1), the lactone monomer is one or more of 4-ethyl-6-methyltetrahydro-2H-pyran-2-one, 4,4,5-trimethyldihydrofuran-2(3H)-one, 3,3,5-trimethyldihydrofuran-2(3H)-one and dibenzo[c,e]oxepin-5(7H)-one; the vulcanizing agent is one or more of Lawesson's reagent, phosphorus pentasulfide and carbon disulfide; and the molar ratio of the lactone monomer to the vulcanizing agent is 1:0.5-1:2.

[0023] Preferably, in step 1), the organic solvent is one or more of tetrahydrofuran, benzene and toluene, and the amount of the organic solvent used per gram of lactone monomer is 10-50 mL; the reflux temperature is 5-10° C. higher than the boiling point of the organic solvent used, and the organic solvent is removed by rotary evaporation under negative pressure at 40-60° C.; the inert atmosphere is one of nitrogen or argon;

[0024] Preferably, in step 1), the chromatographic separation is performed by thin layer chromatography to obtain the best sample R to be separated. f The value is 0.2-0.4, and column chromatography is used for separation, wherein the volume ratio of the weak polar solvent and the strong polar solvent of the mobile phase solvent is 1:1-4:1; the weak polar solvent is one or more of pentane, petroleum ether and n-hexane; the strong polar solvent is one or more of dichloromethane, ethyl acetate and methanol.

[0025] Preferably, in step 2), the vinyl monomer containing an epoxy functional group is one or more of 1-(oxiran-2-yl)propane-2-yl acrylate, 1-(oxiran-2-yl)propyl acrylate, 4-(oxiran-2-yl)butyl-2-yl propionate and oxiran-2-yl methacrylate; the boronic acid monomer is one or more of (3-vinylbenzyl)boric acid, (3-methyl-5-vinylphenylethyl)boric acid, (2-(4-vinylphenyl)propyl)boric acid and (4-vinylphenyl)boric acid; and the molar ratio of the boronic acid monomer to the vinyl monomer containing an epoxy functional group is 1:1-1:2.

[0026] Preferably, in step 2), the inhibitor is one or more of p-methoxyanisole, hydroquinone, 2,6-di-tert-butyl-p-cresol and 2-tert-butylhydroquinone; the mass ratio of the inhibitor to the boric acid monomer is 0.1:100-0.2:100; and the extractant is one or more of ethyl acetate, dichloromethane and diethyl ether.

[0027] Preferably, in step 2), the mass ratio of sulfuric acid to water in the aqueous sulfuric acid solution is 1:100-1.5:100; the addition of anhydrous magnesium sulfate is to remove water in the reaction and promote the reaction to proceed in the forward direction; the neutralization is carried out by adding an alkaline compound to control the pH to 7-7.5; the alkaline compound is one or more of Na2CO3, K2CO3 and NaHCO3; the addition of sodium chloride is to promote salting out; the mass ratio of sodium chloride to boric acid monomer is 1:10-1:5.

[0028] Preferably, in step 2), the molar ratio of anhydrous magnesium sulfate to boric acid monomer is 2:1-5:1; the organic solvent is one or more of ethyl acetate, dichloromethane and diethyl ether, and 10-50 mL of organic solvent is added per gram of boric acid monomer; the purification is to use a low boiling point solvent for washing to remove the raw materials that do not participate in the reaction; the mass ratio of the boric acid monomer to the low boiling point solvent is 1:9-1:2, and the low boiling point solvent is one or more of diethyl ether, petroleum ether, n-pentane, isopentane and n-hexane; the low boiling point solvent is removed after standing for 8-24 hours under negative pressure at 20-40°C.

[0029] Preferably, in step 3), the acrylate monomer is one or more of methyl acrylate, methyl methacrylate, ethyl acrylate, butyl acrylate, tert-butyl acrylate and butyl methacrylate; the mass ratio of the thioester monomer to the acrylate monomer is 1:9-3:7; the mass ratio of the vinyl cross-linking monomer containing a dynamic borate structure and the thioester monomer to the acrylate monomer is 1:100-5:100.

[0030] Preferably, in step 3), the initiator is one or more of potassium persulfate, sodium persulfate and ammonium persulfate; the emulsifier is one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and sodium dodecyl diphenyl oxide disulfonate; the amount of the initiator is 1%-2% of the total mass of the monomers, and the amount of the emulsifier is 1%-2% of the total mass of the monomers; the total mass of the monomers is the sum of the masses of the lactone monomer, the cross-linking monomer containing a dynamic borate structure and the acrylate monomer; the ultrasonic dispersion time is 10-20 min; the stirring speed is 200-300 rpm; the inert atmosphere is one of nitrogen or argon, and the inert atmosphere replacement time is 20-40 min.

[0031] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0032] 1. The dynamic borate structure and thioester bond in the main / side chain degradable acrylate polymer prepared in the present invention can simultaneously give the material excellent mechanical properties and degradability;

[0033] 2. The main / side chain degradable acrylate polymer prepared in the present invention can be degraded by aminolysis, alkaline hydrolysis and oxidative degradation, and the degradation conditions are mild, and the whole process has low energy consumption and little pollution;

[0034] 3. The main / side chain degradable acrylate polymer of the present invention has a simple preparation method and mild synthesis conditions. The solvent used in the preparation process can be reused, and the prepared polymer can be used in high value-added industries. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 1H-NMR nuclear magnetic spectrum of the degradable monomer SDT containing thioester bond;

[0036] Figure 2 1H-NMR image of DVTB, a cross-linking monomer containing a dynamic borate structure;

[0037] Figure 3 ATR infrared spectra of PA / SDT-DVTB polymer of Example 1 and PA / SDT-TGDE polymer of Comparative Example;

[0038] Figure 4 This is the GPC diagram of the degradation product of PA / SDT-DVTB in Example 1;

[0039] Figure 5 The mechanical properties diagram of the polymers of Example 1 PA / SDT-DVTB and Comparative Example PA / SDT-TGDE are shown. DETAILED DESCRIPTION

[0040] In order to better understand the present invention, the present invention is explained below in conjunction with specific embodiments, but the embodiments do not constitute a limitation on the protection scope of the claims of the present invention. Based on the embodiments, other embodiments obtained by those skilled in the art without making any creative work all fall within the protection scope of the present invention.

[0041] The recycling of high-precision instruments such as optoelectronic equipment in high value-added industries is a major problem. The acrylate polymer prepared by the present invention is both degradable and has good mechanical properties. It can replace the polymer products in existing high-precision instruments. It can achieve efficient and environmentally friendly degradation of polymers and recycling of high-precision instruments through simple degradation means, replacing the conventional solvent recovery method on the market. The degradable acrylate polymer prepared by the present invention can be applied to optoelectronic equipment such as printed circuit board (PCB) coating: the coating material used to protect the circuit board requires high precision and good mechanical strength to prevent damage; and after the life of the instrument, it is easy to recycle the circuit board and other components inside the instrument, realizing the recycling of high value-added products.

[0042] From the perspective of polymer molecular structure design, the present invention proposes a main chain / side chain degradable acrylate polymer containing a thioester structure on the main chain and a dynamic borate structure on the side chain, thereby improving the mechanical properties of the main chain degradable acrylate polymer, extending the service life of the material and solving the problem of environmental pollution.

[0043] The thioester monomer used in the present invention is connected to the polymer main chain through free radical ring-opening polymerization, and its structure contains fragile bonds, so under specific conditions, it can be degraded by aminolysis, alkaline hydrolysis and oxidation, and then a cross-linking monomer containing a dynamic borate structure is prepared by dehydration condensation using a boric acid monomer and a vinyl monomer containing a vicinal diol structure as raw materials, and a degradable acrylate polymer prepared by the cross-linking monomer. The dynamic borate structure and the thioester fragile bond have similar degradation conditions, and the cross-linked polymer will not have the phenomenon of small molecule outflow causing the mechanical properties of the material to weaken under normal use, which can improve safety and reliability and extend service life.

[0044] Degradable acrylate polymers introduce degradable fragile thioester bonds into the main chain, which can be broken under specific conditions. They are not only environmentally friendly, but can also be degraded into harmless substances after use, reducing environmental pollution. Dynamic covalent bonds are a type of covalent bond that can be reversibly formed and broken under external stimuli. As a typical dynamic covalent bond, borate bonds have the following characteristics:

[0045] Reversibility: Under certain conditions, the borate ester bond can be broken and reformed, and the dynamic borate ester structure is easily hydrolyzed in the presence of water to generate boronic acid and diol.

[0046] It is sensitive to environmental stimuli (pH value): under alkaline conditions, the boronate ester bond is also easily broken to form borate and the corresponding alcohol.

[0047] Introducing dynamic borate covalent structures into polymer networks can give the materials many excellent properties: under appropriate conditions, the borate bonds can break, allowing the material to degrade into harmless small molecules. The rigid structure of the dynamic borate can also give the material excellent mechanical properties. Therefore, main / side chain degradable acrylate polymers containing thioester and dynamic borate structures are of great significance in solving the problem of plastic pollution and promoting the development of sustainable materials.

[0048] The main and side chain degradable polymers of the present invention with dynamic crosslinking can have higher tensile strength, because the crosslinking structure can disperse stress more effectively, and due to the network structure provided by the crosslinking points, generally have higher modulus and higher fracture toughness, attributed to the dynamic crosslinking structure can effectively resist crack propagation. The polymer has excellent mechanical properties, and can degrade and repair mechanical damage under appropriate conditions, reducing resource waste and environmental pollution.

[0049] When preparing the main / side chain degradable acrylic ester polymer containing thioester and dynamic borate structures of the present invention, a thioester monomer containing a fragile bond is first synthesized, and is connected to the main chain of the acrylic ester polymer through free radical ring-opening polymerization, so that the polymer has degradable performance; then, a crosslinking monomer containing a dynamic borate structure is prepared by dehydration condensation using boric acid monomers and vinyl monomers containing vicinal diol structures as raw materials, so that the polymer realizes dynamic crosslinking; and then, the thioester monomer, the crosslinking monomer containing the dynamic borate structure and the acrylic ester monomer are polymerized to obtain the main / side chain degradable acrylic ester polymer containing thioester and dynamic borate structures.

[0050] The method for preparing the main / side chain degradable acrylate polymer containing thioester and dynamic borate structure of the present invention specifically comprises the following steps:

[0051] 1) dissolving the lactone monomer in an organic solvent free of water, adding a vulcanizing agent, stirring and reacting for 5-8 hours under an inert atmosphere, removing the organic solvent, and separating by chromatography to obtain a thioester monomer;

[0052] 2) adding a vinyl monomer containing an epoxy functional group and a polymerization inhibitor to a sulfuric acid aqueous solution, stirring the obtained mixture at 70-80° C. for 2-4 hours, and cooling to room temperature; adding sodium chloride after neutralization, extracting the mixture, and distilling under reduced pressure to obtain a vinyl monomer containing a vicinal diol structure; dissolving the obtained product in an organic solvent, adding a boric acid monomer and anhydrous magnesium sulfate, stirring and reacting at room temperature for 12-24 hours, then heating to 40-60° C. and distilling under reduced pressure to remove the organic solvent described in this step, and purifying to obtain a vinyl cross-linking monomer containing a dynamic borate ester structure;

[0053] 3) After mixing deionized water, an initiator and an emulsifier, the air is replaced under an inert atmosphere; after adding a thioester monomer, a vinyl crosslinking monomer containing a dynamic borate structure and an acrylate monomer, the mixture is ultrasonically dispersed, and the mixture is stirred and reacted at 70-80° C. to obtain a main / side chain degradable acrylate polymer containing a thioester and a dynamic borate structure.

[0054] The main / side chain degradable acrylate polymer containing thioester and dynamic borate structure of the present invention has the following structural formula:

[0055]

[0056] Wherein m1, m2, m3, m4 = 30-36, n1, n2, n3, n4 = 24-29;

[0057] R1 is one of the following groups:

[0058]

[0059] R2 is one of the following groups:

[0060]

[0061] R3 is one of the following groups:

[0062]

[0063] Based on the main / side chain degradable acrylate polymer structural formula containing thioester and dynamic borate structure of the present invention, the lactone monomer, vinyl monomer containing epoxy functional group, boric acid monomer, thioester monomer and acrylate monomer involved in its preparation method can be selected according to the purpose of the invention; as for the auxiliary raw materials such as organic solvent, vulcanizing agent, initiator and emulsifier, they can be selected according to the dissolution requirements, vulcanization requirements and the initiation and emulsification requirements of this type of reaction.

[0064] The relevant testing methods in the embodiments of the present invention are as follows:

[0065] Nuclear Magnetic Resonance (NMR): 1H spectra were recorded at 25°C on a Bruker Avance III 400 MHz spectrometer (1H: 400 MHz). The samples were dissolved in CDCl3 at approximately 30 mg mL -1 The NMR spectra were recorded using a 5 mm BBFO+ probe with a z-gradient coil.

[0066] Fourier transform infrared spectroscopy (FTIR) test: For bulk polymer film samples, the attenuated total reflectance (ATR) accessory is used to directly test the elastic film after film formation. The Fourier transform infrared spectroscopy test range is 4000cm -1 Up to 400cm -1 , resolution 4cm -1 , the number of scans is 32 times.

[0067] GPC analysis: SEC analysis was performed using a Viscotek system (Malvern Instruments) consisting of a four-capillary differential viscometer, a differential refractive index (RI) detector, and a UV detector. THF was used as the mobile phase at a flow rate of 1 mL min -1 , 35 °C. After filtration through a 0.45 μm PTFE membrane, the -1 All samples were injected at a concentration of . Separation was performed on three polymer standard service columns (SDVB, 5 μm, 300×7.5 mm) and a guard column. The average molar mass (number average molar mass, Mn and weight average molar mass, Mw) and molar mass dispersion,

[0068] Mechanical properties test: The mechanical properties of the samples were characterized using a universal material testing machine. The sample films with a thickness of 0.9-1.2 mm were cut into 4 dumbbell-shaped specimens according to the national standard GB / T 528-2009, with a size of 2×35 mm, a gauge length of 12 mm, and a tensile rate of 500 mm min. -1 , the test temperature is 23±2℃, the humidity is 60±10%, each sample is repeated at least 3 times and the average value is taken.

[0069] Example 1

[0070] A method for preparing a main / side chain degradable acrylic ester polymer PA / SDT-DVTB containing a thioester and a dynamic borate ester structure, comprising the following steps:

[0071] Synthesis and purification of thioester monomer: 10.54 g of dibenzo[c,e]oxepin-5(7H)-one was dissolved in 60 mL of toluene, and then 32.32 g of Lawesson reagent was slowly added. The mixed dispersion was stirred under a nitrogen atmosphere, heated to 115°C, condensed and refluxed for 7 h, and then toluene was removed by rotary evaporation to obtain a viscous liquid. The best sample to be separated R was obtained by thin layer chromatography. fThe value is 0.4, and the ratio of the mobile phase is n-hexane (weak polar solvent): dichloromethane (strong polar solvent) = 2:1. The above viscous liquid is separated by column chromatography using silica gel powder as an adsorbent, and then the mobile phase solvent is removed by reduced pressure distillation to obtain a degradable monomer containing a thioester bond, dibenzo[c,e]oxepene-5(7H)-thione (SDT), with a yield of 35% (yield = 100% × actual production of the target product / theoretical production of the target product). The 1H-NMR nuclear magnetic spectrum of SDT is obtained by testing with a Bruker Avance III 400MHz spectrometer, and the 1H-NMR nuclear magnetic spectrum of the DOT monomer is as follows: Figure 1 The successful synthesis of SDT was confirmed. 1HNMR (500MHz, Chloroform-d) δ8.18 (d, J = 8.9 Hz, 1H), 7.67 (d, J = 7.7 Hz, 2H), 7.62 (t, J = 6.9 Hz, 1H), 7.58-7.51 (m, 2H), 7.47 (d, J = 4.9 Hz, 2H), 5.20 (d, J = 24.1 Hz, 2H).

[0072] Synthesis and purification of borate monomer: 60g of oxirane-2-yl methacrylate and 0.06g of p-methoxyanisole were added to 180g of aqueous solution containing 2g of sulfuric acid, stirred at 80°C for 2h, and cooled to room temperature. First, 4g of Na2CO3 was added to neutralize the excess acid in the reaction, and then 5g of sodium chloride was added to promote salting out, accelerate the separation of the aqueous phase and the organic phase, inhibit the formation of the emulsion layer, and improve the extraction rate. The mixture was extracted with 250mL of ethyl acetate, and the extraction was repeated three times. 5g of anhydrous magnesium sulfate was added to remove the water in the ethyl acetate. After the ethyl acetate was removed by vacuum distillation, the vinyl monomer 2,3-dihydroxypropyl methacrylate containing a vicinal diol structure was obtained. 18g of (4-vinylphenyl)boric acid was dissolved in 200mL of tetrahydrofuran, and 12.6g of 2,3-dihydroxypropyl methacrylate was slowly added dropwise. 14g of anhydrous magnesium sulfate was added and stirred at room temperature for 12h. The magnesium sulfate was then filtered to remove the mixed solution. The mixture was then heated to 55°C and the tetrahydrofuran was removed by vacuum distillation to obtain a viscous liquid. The mixture was then washed with ether. The colorless viscous liquid obtained after removing the raw materials that did not participate in the reaction was the vinyl cross-linking monomer (2-(4-vinylphenyl)-1,3,2-dioxaborane-4-yl) methacrylate (DVTB) containing a dynamic borate structure. The yield was 88% (yield = 100% × actual production of the target product / theoretical production of the target product). The 1H-NMR nuclear magnetic spectrum of DVTB was obtained by testing with a Bruker Avance III 400MHz spectrometer, as shown in FIG. Figure 2The successful synthesis of DVTB was confirmed. 1H NMR (600MHz, Chloroform-d) δ7.84–7.73 (m, 2H), 7.48–7.38 (m, 2H), 6.73 (dd, J=17.6, 10.9 Hz, 1H), 6.16–6.05 (m, 1H), 5.88–5.77 (m, 1H), 5.61–5.51 (m, 1H), 5.37–5.25 (m, 1H), 4.84 (ddt, J=8.3, 6.1, 4.2 Hz, 1H), 4.52–4.14 (m, 4H), 1.94–1.88 (m, 3H).

[0073] Preparation of main / side chain degradable acrylate polymer containing thioester and dynamic borate structure: 40g deionized water, 0.15g initiator potassium persulfate (KPS, 1.5wt.% vs monomer, the total mass of monomers is the sum of SDT monomer, DVTB monomer and acrylate monomer) and 0.2g emulsifier sodium dodecyl sulfate (SDS, 2.0wt.% vs monomer, the total mass of monomers is the sum of SDT monomer, DVTB monomer and acrylate monomer) were added to a 50mL flask, nitrogen was replaced for 20min, and then 0.9g SDT, 0.3g DVTB and 8.8g acrylate monomer (4.4g methyl methacrylate, 4.4g butyl acrylate) were added. After stirring at 70°C and 250rpm for 4h, the main / side chain degradable acrylate polymer PA / SDT-DVTB (20wt.%) containing thioester and dynamic borate structure was obtained. The polymers of Example 1 PA / SDT-DVTB and Comparative Example PA / SDT-TGDE were tested by Fourier transform infrared spectroscopy (FTIR). The ATR infrared spectra were as follows: Figure 3 Shown: 1686cm -1 The stretching vibration peak of -SC=O at 1606 cm -1 The stretching vibration peak representing the borate ester bond proves that the DVTB monomer is incorporated into the polymer side chain, thus confirming the successful preparation of PA / SDT-DVTB polymer.

[0074] The relevant proofs of the following examples regarding borate monomers, borate monomers, and main / side chain degradable acrylate polymers containing thioester and dynamic borate structures are similar and are not provided one by one.

[0075] Example 2

[0076] A method for preparing a main / side chain degradable acrylic ester polymer PA / TDT-EDMP containing a thioester and a dynamic borate ester structure, comprising the following steps:

[0077] Synthesis and purification of thioester monomer: 11.54 g of 4,4,5-trimethyldihydrofuran-2(3H)-one was dissolved in 80 mL of benzene, and then 22.21 g of phosphorus pentasulfide reagent was slowly added. The mixed dispersion was stirred under an argon atmosphere, heated to 85°C, condensed and refluxed for 6 hours. After the end, most of the organic solvent was removed by rotary evaporation, and the remaining viscous liquid was separated by column chromatography, and the best sample R to be separated was obtained by thin layer chromatography. f The value is 0.3, and the ratio of the mobile phase is n-hexane (weak polar solvent): ethyl acetate (strong polar solvent) = 3:1. The above products are separated by column chromatography using alumina as an adsorbent to obtain a clear solution. The clear solution is then heated to 60°C and the mobile phase solvent is removed by reduced pressure distillation to obtain a degradable monomer containing a thioester bond, 4,4,5-trimethyldihydrofuran-2(3H)-thione (TDT), with a yield of 57% (yield = 100% × actual production of the target product / theoretical production of the target product).

[0078] Synthesis and purification of borate monomer: 40g of 1-(oxirane-2-yl)propyl acrylate and 0.04g of 2,6-di-tert-butyl toluene were added to 150g of aqueous solution containing 1.5g of sulfuric acid, stirred at 70°C for 4h, and cooled to room temperature. First, 5g of K2CO3 was added to neutralize the excess acid in the reaction, and then 7g of sodium chloride was added to promote salting out, accelerate the separation of the aqueous phase and the organic phase, inhibit the formation of the emulsion layer, and improve the extraction rate. The mixture was extracted with 280mL of ethyl acetate, and the extraction was repeated three times. 5g of anhydrous magnesium sulfate was added to remove the water in the ethyl acetate. After the ethyl acetate was removed by vacuum distillation, the vinyl monomer 1,2-dihydroxypentane-3-yl acrylate containing a vicinal diol structure was obtained, which was a colorless viscous liquid. 16 g of (3-methyl-5-vinylphenethyl)boric acid was dissolved in 300 mL of tetrahydrofuran, 13.4 g of 1,2-dihydroxypentane-3-yl acrylate was slowly added dropwise, and then 12 g of anhydrous magnesium sulfate was added. After stirring at room temperature for 12 h, the magnesium sulfate was removed by filtration to obtain a mixed solution containing borate ester; the mixed solution was heated to 55° C. and tetrahydrofuran was removed by reduced pressure distillation, and then washed with ether to obtain a vinyl cross-linking monomer 1-(2-(3-methyl-5-vinylphenethyl)-1,3,2-dioxaborolan-4-yl)propyl acrylate (EDMP) containing a dynamic borate ester structure, and the yield was 80% (yield = 100% × actual production amount of the target product / theoretical production amount of the target product).

[0079] Preparation of main / side chain degradable acrylate polymer containing thioester and dynamic borate structure: 40g deionized water, 0.1g initiator ammonium persulfate (NH4PS, 1.0wt.% vs monomer, the total mass of monomers is the sum of TDT monomer, EDMP monomer and acrylate monomer) and 0.15g emulsifier sodium dodecylbenzene sulfonate (SDBS, 1.5wt.% vs monomer, the total mass of monomers is the sum of TDT monomer, EDMP monomer and acrylate monomer) were added to a 50mL flask, argon gas was replaced for 30min, and then 1.3g TDT, 0.3g EDMP and 8.4g acrylate monomer (4.2g methyl methacrylate, 4.2g ethyl acrylate) were added. After stirring at 80°C and 250rpm for 4h, the main / side chain degradable acrylate polymer PA / TDT-EDMP (20wt.%) containing thioester and dynamic borate structure was obtained.

[0080] Example 3

[0081] A method for preparing a main / side chain degradable acrylate polymer PA / DMT-PDMP containing a thioester and a dynamic borate structure, comprising the following steps:

[0082] Synthesis and purification of thioester monomer: 9.68 g of 3,3,5-trimethyldihydrofuran-2(3H)-one was dissolved in 90 mL of tetrahydrofuran, and then 9.12 g of carbon disulfide reagent was slowly added. The mixed dispersion was stirred under a nitrogen atmosphere, heated to 75°C, condensed and refluxed for 5 h, and tetrahydrofuran was removed by rotary evaporation to obtain a reaction mixture. The best sample to be separated R was obtained by thin layer chromatography. f The value is 0.3, and the mobile phase ratio is petroleum ether (weak polar solvent): ethyl acetate (strong polar solvent) = 2:1. The viscous liquid is separated by column chromatography using aluminum oxide as an adsorbent to obtain a clear solution. The clear solution is heated to 50°C and the mobile phase solvent is removed by vacuum distillation to obtain a degradable monomer containing a thioester bond, 3,3,5-trimethyldihydrofuran-2(3H)-thione (DMT), with a yield of 38% (yield = 100% × actual production of the target product / theoretical production of the target product).

[0083] Synthesis and purification of borate monomer: 50g of 4-(oxirane-2-yl)butan-2-yl acrylate and 0.05g of hydroquinone were added to 200g of aqueous solution containing 2g of sulfuric acid. The mixture was stirred at 80°C for 4h and cooled to room temperature. First, 4g of NaHCO3 was added to neutralize the excess acid in the reaction, and then 8g of sodium chloride was added to promote salting out, accelerate the separation of the aqueous phase and the organic phase, inhibit the formation of the emulsion layer, and improve the extraction rate. The mixture was extracted with 300mL of ethyl acetate, and the extraction was repeated three times. 5g of anhydrous magnesium sulfate was added to remove the water in the ethyl acetate. After the ethyl acetate was removed by vacuum distillation, the vinyl monomer 5,6-dihydroxyhexane-2-yl acrylate containing a vicinal diol structure was obtained, which was a colorless viscous liquid. 14 g of (2-(4-vinylphenyl)propyl)boric acid was dissolved in 300 mL of tetrahydrofuran, 18.4 g of 5,6-dihydroxyhexane-2-yl acrylate was slowly added dropwise, and then 10 g of anhydrous magnesium sulfate was added. The mixed dispersion was stirred at room temperature for 12 hours and then filtered to remove the magnesium sulfate to obtain a clear mixed solution containing borate ester; the mixed solution was heated to 45° C. and the organic solvent was removed by distillation under reduced pressure to obtain a viscous liquid, which was a vinyl cross-linking monomer containing a dynamic borate ester structure, 4-(2-(2-(4-vinylphenyl)propyl)-1,3,2-dioxaborolane-4-yl)butane-2-yl methacrylate (PDMP), and the yield was 86% (yield = 100% × actual production amount of the target product / theoretical production amount of the target product)

[0084] Preparation of main / side chain degradable acrylate polymer containing thioester and dynamic borate structure: 40g deionized water, 0.15g initiator sodium persulfate (NaPS, 1.5wt.% vs monomer, the total mass of monomers is the sum of DMT monomer, PDMP monomer and acrylate monomer) and 0.15g emulsifier sodium dodecyl diphenyl ether disulfonate (SLDED, 1.5wt.% vs monomer, the total mass of monomers is the sum of DMT monomer, PDMP monomer and acrylate monomer) were added to a 50mL flask, nitrogen replacement for 20min, and then 1g DMT, 0.3g PDMP and 8.7g acrylate monomer (4.5g methyl methacrylate, 4.2g tert-butyl acrylate) were added. After stirring at 70°C and 250rpm for 4h, the main / side chain degradable acrylate polymer PA / DMT-PDMP (20wt.%) containing thioester and dynamic borate structure was obtained.

[0085] Example 4

[0086] A method for preparing a main / side chain degradable acrylic ester polymer PA / EMPT-EMBP containing a thioester and a dynamic borate ester structure, comprising the following steps:

[0087] Synthesis and purification of thioester monomer: 16.42 g of 4-ethyl-6-methyltetrahydro-2H-pyran-2-one was dissolved in 100 mL of toluene, and then 24.22 g of Lawesson reagent was slowly added. The mixed dispersion was stirred under an argon atmosphere, heated to 115 ° C, condensed and refluxed for 6 hours. After the end, toluene was removed by rotary evaporation to obtain a viscous liquid. The best sample R to be separated was obtained by thin layer chromatography f The value is 0.3, and the ratio of the mobile phase is n-hexane (weak polar solvent): dichloromethane (strong polar solvent) = 3:1. The viscous liquid is separated by column chromatography using silica gel powder as an adsorbent to obtain a clear solution. The clear solution is heated to 90°C and the mobile phase solvent is removed by vacuum distillation to obtain a degradable monomer containing a thioester bond, 4-ethyl-6-methyltetrahydro-2H-pyran-2-thione (EMPT), with a yield of 45% (yield = 100% × actual production amount of the target product / theoretical production amount of the target product).

[0088] Synthesis and purification of vinyl cross-linked monomers containing dynamic borate structures: 30 g of 1-(oxirane-2-yl)propane-2-yl acrylate and 0.03 g of p-methoxyanisole were added to 200 g of aqueous solution containing 2.5 g of sulfuric acid, and the ring was opened by acidic catalysis. The mixture was stirred at 80 ° C for 2 h and cooled to room temperature. First, 3 g of Na2CO3 was added to neutralize the excess acid in the reaction, and then 5 g of sodium chloride was added to promote salting out, accelerate the separation of the aqueous phase and the organic phase, inhibit the formation of the emulsion layer, and improve the extraction rate. The mixture was extracted with 200 mL of ethyl acetate, and the extraction was repeated three times. 5 g of anhydrous magnesium sulfate was added to remove the water in the ethyl acetate. After the ethyl acetate was removed by reduced pressure distillation, 4,5-dihydroxypentan-2-yl acrylate containing vicinal diol was obtained as a colorless viscous liquid.

[0089] 18g of (3-vinylbenzyl)boric acid was dissolved in 200mL of tetrahydrofuran, 14.8g of 4,5-dihydroxypentan-2-yl acrylate was slowly added dropwise, and then 10g of anhydrous magnesium sulfate was added. The mixed dispersion was stirred at room temperature for 12h and then filtered to remove the magnesium sulfate to obtain a clear mixed solution containing borate ester; the mixed solution was heated to 50°C, and the organic solvent was removed by reduced pressure distillation, and then the raw materials that did not participate in the reaction were washed with ether to remove the raw materials, and then a vinyl cross-linking monomer 1-(2-(3-vinylbenzyl)-1,3,2-dioxaborane-4-yl)propane-2-yl acrylate (EMBP) containing a dynamic borate ester structure was obtained. The yield was 85% (yield = 100% × actual production amount of the target product / theoretical production amount of the target product)

[0090] Preparation of main / side chain degradable acrylate polymer containing thioester and dynamic borate structure: 40g deionized water, 0.2g initiator NaPS (2.0wt.% vs monomer, the total mass of monomers is the sum of EMPT monomer, EMBP monomer and acrylate monomer) and 0.15g emulsifier SDBS (1.5wt.% vs monomer, the total mass of monomers is the sum of EMPT monomer, EMBP monomer and acrylate monomer) were added to a 50mL flask, argon gas was replaced for 25min, and then 0.9g EMPT, 0.3g EMBP and 8.8g acrylate monomer (4.4g methyl methacrylate, 4.4g methyl acrylate) were added. After stirring at 250rpm at 75°C for 4h, the main / side chain degradable acrylate polymer PA / EMPT-EMBP (20wt.%) containing thioester and dynamic borate structure was obtained.

[0091] Comparative Example

[0092] A method for preparing a degradable acrylate cross-linked polymer PA / SDT-TGDE containing a non-dynamic covalent structure comprises the following steps:

[0093] Synthesis and purification of thioester monomer: 8.44 g of dibenzo[c,e]oxepin-5(7H)-one was dissolved in 40 g of toluene, and then 25.86 g of Lawesson reagent was slowly added. The mixed dispersion was stirred under a nitrogen atmosphere, heated to 115°C, condensed and refluxed for 5 h, and then toluene was removed by rotary evaporation to obtain a viscous liquid. The best sample to be separated R was obtained by thin layer chromatography. f The value is 0.4, and the ratio of the mobile phase is n-hexane (weakly polar solvent): dichloromethane (strongly polar solvent) = 1:2. The viscous liquid is separated by column chromatography using silica gel powder as an adsorbent, and then the mobile phase solvent is removed by reduced pressure distillation to obtain a degradable monomer SDT containing a thioester bond.

[0094] Preparation of degradable acrylate cross-linked polymer containing non-dynamic covalent bonds: 40g deionized water, 0.15g initiator KPS (1.5wt.% vs monomer) and 0.2g emulsifier SDS (2.0wt.% vs monomer) were added to a 50mL flask, nitrogen replaced for 20min, and then 0.8g SDT, 0.3g triethylene glycol divinyl ether (TGDE) and 8.9g acrylate monomer (4.5g methyl methacrylate, 4.4g butyl acrylate) were added. After stirring at 70°C and 250rpm for 4h, a degradable acrylate polymer PA / SDT-TGDE (20wt.%) containing a non-dynamic covalent structure was obtained.

[0095] The polymers of Example 1 PA / SDT-DVTB and Comparative Example PA / SDT-TGDE were tested by Fourier transform infrared spectroscopy (FTIR). The ATR infrared spectra were as follows: Figure 3 Shown: 1686cm -1 The stretching vibration peak of -SC=O at 1606 cm -1 The stretching vibration peak at 1686 cm represents the borate ester bond, proving that the DVTB monomer is incorporated into the polymer side chain, thus confirming the successful preparation of the PA / SDT-DVTB polymer. -1 The stretching vibration peak of -SC=O at position proves that the SDT monomer is successfully incorporated into the main chain of the polymer PA / SDT-TGDE, and the polymer is insoluble in THF, indicating that the cross-linked structure is also successfully prepared.

[0096] The GPC graph of the degradation products of PA / SDT-DVTB in Example 1 under different degradation conditions is shown in FIG. Figure 4 As shown, under the alkaline and aminolysis conditions of PA / SDT-DVTB polymer, the polymer cross-linking structure is interrupted and the polymer molecular weight is reduced. The products obtained in Example 1 and the comparative example were placed in 0.1mol / L KOH solution and 0.1mol / L IPA solution for degradation tests under alkaline and aminolysis conditions, and the results are shown in Table 1. The thioester bond and dynamic borate structure in the PA / SDT-DVTB polymer of Example 1 are broken under alkaline and aminolysis conditions, and the polymer cross-linking structure is interrupted into a straight chain structure, and the polymer molecular weight is reduced. The number average molecular weight of the polymer after degradation under alkaline and aminolysis conditions is 9346.4g / mol and 7929.6g / mol respectively; the weight average molecular weight of the PA / SDT-DVTB polymer after degradation under alkaline and aminolysis conditions is 25796.1g / mol and 18475.9g / mol respectively, and the polymer dispersity of the PA / SDT-DVTB polymer of Example 1 after degradation under alkaline and aminolysis conditions is 2.765 and 2.334 respectively.

[0097] Degradation rate: Degradation rate is used to measure the degree of decomposition or degradation of a substance under certain conditions. The formula for calculating degradation rate is as follows: Degradation rate (%) = ((initial weight - final weight) / initial weight) × 100%

[0098] The specific steps for calculating the degradation rate are as follows:

[0099] 1. Measure initial weight: Accurately measure the initial weight of the test material before testing.

[0100] 2. Degradation test: Place the test substance under degradation conditions for a certain period of time (the time is determined according to the degradation conditions).

[0101] 3. Measure the final weight: After the degradation experiment is completed, take out the test material and measure its final weight.

[0102] 4. Calculate the degradation rate: According to the above formula, calculate the degradation rate of the test substance.

[0103] The PA / SDT-DVTB polymer obtained in Example 1 achieved a degradation rate of 90% and 99% under alkaline hydrolysis and aminolysis conditions, respectively, within 24 hours. The degradation effect of PA / SDT-DVTB polymer under aminolysis conditions is better than that under alkaline degradation conditions, indicating that the degradable structural units are more sensitive to aminolysis. The comparative PA / SDT-TGDE polymer achieved a degradation rate of less than 5% after 24 hours, wherein a small amount of degradable fragments came from the structure in which the polymer contained part that was not locked by the cross-linked structure and the thioester unit on the main chain was degradable, while more than 95% of the part was locked by the non-degradable cross-linked structure and could not be degraded. The experimental results show that the PA / SDT-DVTB polymer containing borate ester can achieve a higher degradation rate under mild conditions (low-concentration alkaline environment), which is beneficial to reduce the pollution to the environment after the material is damaged and discarded.

[0104] Table 1 Degradation (alkaline hydrolysis-KOH and aminolysis-IPA) data of Example 1 and Comparative Example

[0105]

[0106] The mechanical properties of Example 1 PA / SDT-DVTB and Comparative Example PA / SDT-TGDE were characterized using a universal material testing machine. Figure 5 As shown: the tensile strength and elongation at break of the comparative example PA / SDT-TGDE polymer are 3.27 MPa and 228.6% respectively, and the tensile strength and elongation at break of the example 1 PA / SDT-TGDE polymer are 7.87 MPa and 403.7% respectively, and its mechanical properties are significantly improved, which are better than those of the TGDE non-dynamically cross-linked polymer, indicating that the rigid structure of the DVTB-cross-linked borate ester greatly improves the mechanical properties of the polymer.

[0107] Traditional acrylate polymers are difficult to degrade in the environment due to their structural stability, resulting in serious plastic pollution problems. The present invention prepares a chemically degradable PA / SDT-DVTB polymer containing a thioester and a dynamic borate structure, which is easy to degrade under mild conditions due to the chemical sensitivity of the thioester and dynamic borate structures in its composition, thereby reducing the pollution to the environment after the material is discarded. In addition, the present invention also greatly improves the mechanical properties of the polymer PA / SDT-DVTB through the cross-linking of the dynamic borate structure monomer DVTB, so that it has excellent mechanical properties, can meet a wide range of application scenarios, is conducive to improving the safety and reliability of the material and extending its service life, which is far superior to the TGDE cross-linked polymer. The degradable PA / SDT-DVTB polymer prepared by the present invention has excellent mechanical properties and can be applied to high-precision instruments such as optoelectronic devices with mechanical performance requirements, and the mild degradation conditions of the polymer are conducive to the degradation of acrylate materials in the housing and internal structural parts of optoelectronic devices such as electronic printed circuit boards (PCBs), thereby realizing the reuse of circuit boards.

[0108] The implementation methods of the present invention are not limited to the above-mentioned embodiments, and any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.

Claims

1. A main / side chain degradable acrylic polymer containing a thioester and a dynamic borate structure, characterized in that Has the following structural formula: Wherein m1, m2, m3, m4 = 30-36, n1, n2, n3, n4 = 24-29; R1 is one of the following groups: R2 is one of the following groups: R3 is one of the following groups:

2. The method for preparing a main / side chain degradable acrylate polymer containing a thioester and a dynamic borate structure according to claim 1, characterized in that The steps include: 1) dissolving the lactone monomer in an organic solvent free of water, adding a vulcanizing agent, stirring and reacting for 5-8 hours under an inert atmosphere, removing the organic solvent, and separating by chromatography to obtain a thioester monomer; 2) adding a vinyl monomer containing an epoxy functional group and a polymerization inhibitor to a sulfuric acid aqueous solution, stirring the resulting mixture at 70-80° C. for 2-4 hours, and cooling to room temperature; adding sodium chloride after neutralization, extracting the mixture, and distilling under reduced pressure to obtain a vinyl monomer containing a vicinal diol structure; dissolving the resulting product in an organic solvent, adding a boric acid monomer and anhydrous magnesium sulfate, stirring and reacting at room temperature for 12-24 hours, then heating to 40-60° C. and distilling under reduced pressure, and purifying to obtain a vinyl cross-linking monomer containing a dynamic borate ester structure; 3) After mixing deionized water, an initiator and an emulsifier, the air is replaced under an inert atmosphere; after adding a thioester monomer, a vinyl crosslinking monomer containing a dynamic borate structure and an acrylate monomer, the mixture is ultrasonically dispersed, and the mixture is stirred and reacted at 70-80° C. to obtain a main / side chain degradable acrylate polymer containing a thioester and a dynamic borate structure.

3. The method for preparing the main / side chain degradable acrylate polymer containing thioester and dynamic borate structure according to claim 2, characterized in that: In step 1), the lactone monomer is one or more of 4-ethyl-6-methyltetrahydro-2H-pyran-2-one, 4,4,5-trimethyldihydrofuran-2(3H)-one, 3,3,5-trimethyldihydrofuran-2(3H)-one and dibenzo[c,e]oxepin-5(7H)-one; the vulcanizing agent is one or more of Lawesson's reagent, phosphorus pentasulfide and carbon disulfide; the molar ratio of the lactone monomer to the vulcanizing agent is 1:0.5-1:

2.

4. The method for preparing the main / side chain degradable acrylate polymer containing thioester and dynamic borate structure according to claim 2, characterized in that: In step 1), the organic solvent is one or more of tetrahydrofuran, benzene and toluene, and the amount of the organic solvent used per gram of lactone monomer is 10-50 mL; the reflux temperature is 5-10° C. higher than the boiling point of the organic solvent used, and the organic solvent is removed by rotary evaporation under negative pressure at 40-60° C.; the inert atmosphere is one of nitrogen or argon; The chromatographic separation is to obtain the best sample R to be separated by thin layer chromatography. f The value is 0.2-0.4, and column chromatography is used for separation, wherein the volume ratio of the weak polar solvent and the strong polar solvent of the mobile phase solvent is 1:1-4:1; the weak polar solvent is one or more of pentane, petroleum ether and n-hexane; the strong polar solvent is one or more of dichloromethane, ethyl acetate and methanol.

5. The method for preparing the main / side chain degradable acrylate polymer containing thioester and dynamic borate structure according to claim 2, characterized in that: In step 2), the vinyl monomer containing an epoxy functional group is one or more of 1-(oxiran-2-yl)propane-2-yl acrylate, 1-(oxiran-2-yl)propyl acrylate, 4-(oxiran-2-yl)butyl-2-yl propionate and oxiran-2-yl methacrylate; the boronic acid monomer is one or more of (3-vinylbenzyl)boric acid, (3-methyl-5-vinylphenylethyl)boric acid, (2-(4-vinylphenyl)propyl)boric acid and (4-vinylphenyl)boric acid; the molar ratio of the boronic acid monomer to the vinyl monomer containing an epoxy functional group is 1:1-1:

2.

6. The method for preparing the main / side chain degradable acrylate polymer containing thioester and dynamic borate structure according to claim 2, characterized in that: In step 2), the inhibitor is one or more of p-methoxyanisole, hydroquinone, 2,6-di-tert-butyl-p-cresol and 2-tert-butylhydroquinone; the mass ratio of the inhibitor to the boric acid monomer is 0.1:100-0.2:100; and the extractant is one or more of ethyl acetate, dichloromethane and diethyl ether.

7. The method for preparing the main / side chain degradable acrylate polymer containing thioester and dynamic borate structure according to claim 2, characterized in that: In step 2), the mass ratio of sulfuric acid to water in the aqueous sulfuric acid solution is 1:100-1.5:100; the addition of anhydrous magnesium sulfate is to remove water in the reaction and promote the reaction to proceed in the forward direction; the neutralization is carried out by adding an alkaline compound to control the pH to 7-7.5; the alkaline compound is one or more of Na2CO3, K2CO3 and NaHCO3; the addition of sodium chloride is to promote salting out; the mass ratio of sodium chloride to boric acid monomer is 1:10-1:

5.

8. The method for preparing the main / side chain degradable acrylate polymer containing thioester and dynamic borate structure according to claim 7, characterized in that: In step 2), the molar ratio of anhydrous magnesium sulfate to boric acid monomer is 2:1-5:1; the organic solvent is one or more of ethyl acetate, dichloromethane and diethyl ether, and 10-50 mL of organic solvent is added per gram of boric acid monomer; the purification is to use a low boiling point solvent to wash and remove the raw materials that do not participate in the reaction; the mass ratio of the boric acid monomer to the low boiling point solvent is 1:9-1:2, and the low boiling point solvent is one or more of diethyl ether, petroleum ether, n-pentane, isopentane and n-hexane; the low boiling point solvent is removed after standing for 8-24 hours under negative pressure at 20-40°C.

9. The method for preparing the main / side chain degradable acrylate polymer containing thioester and dynamic borate structure according to claim 2, characterized in that: In step 3), the acrylate monomer is one or more of methyl acrylate, methyl methacrylate, ethyl acrylate, butyl acrylate, tert-butyl acrylate and butyl methacrylate; the mass ratio of the thioester monomer to the acrylate monomer is 1:9-3:7; the mass ratio of the vinyl cross-linking monomer containing a dynamic borate structure and the thioester monomer to the acrylate monomer is 1:100-5:

100.

10. The method for preparing the main / side chain degradable acrylate polymer containing thioester and dynamic borate structure according to claim 2, characterized in that: In step 3), the initiator is one or more of potassium persulfate, sodium persulfate and ammonium persulfate; the emulsifier is one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and sodium dodecyl diphenyl ether disulfonate; the amount of the initiator is 1%-2% of the total weight of the monomers, and the amount of the emulsifier is 1%-2% of the total weight of the monomers; the total weight of the monomers is lactone monomers, crosslinking monomers containing dynamic borate structures and acrylic acid The total mass of the ester monomers; the ultrasonic dispersion time is 10-20min; the stirring speed is 200-300rpm; The inert atmosphere is one of nitrogen or argon, and the time for replacing the inert atmosphere is 20-40 minutes.

Citation Information

Patent Citations

  • Dynamic polymer having hybrid cross-linked network and application thereof

    CN107805308A

  • Polymer compositions comprising cross-linked polymers comprising boronic ester functions enabling exchange reactions, process for preparing them and their use

    CN111410711A

  • Degradable crosslinker for (METH) acrylic resin and method thereof

    CN118355040A

Cited By

  • Degradable mobile phone gum material and preparation process thereof

    CN120082305A

  • Slow-release medicinal enteric-coated material and preparation method thereof

    CN120899930A