Manufacturing method of polyurethane foam material

Through the combination of high-active polyether and plant-based modified MDI, high-pressure gun head injection molding is used to solve the shortcomings of the acoustic performance and environmentally friendly materials of polyurethane foaming materials, and the acoustic performance improvement and carbon emission reduction are achieved. Complex and simple carpet production.

CN118909219APending Publication Date: 2024-11-08YI QI SI HUAN QI YE ZONG GONG SI FU LI CHANG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411135891.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing polyurethane foaming materials have shortcomings in acoustic performance and environmentally friendly materials, and it is difficult to achieve excellent acoustic performance and low-carbon environmental protection goals at the same time.

Method used

Using high-active polyether, slow rebound polyether, PET recovery polyether, stabilizer, catalyst, crosslinking agent, aldehyde removal agent and pore opening agent, it is molded through high-pressure gun tip injection mold, combined with plant-based modified MDI , prepare polyurethane foaming materials with good acoustic performance.

Benefits of technology

It significantly improves the acoustic performance of the material and reduces carbon emissions. It is suitable for carpet production with complex shapes and long-term pouring. It is also compatible with carpet production with simple structures and good raw material compatibility.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of a polyurethane foam material. The polyurethane foam material is prepared from the following raw materials in parts by weight: 40-60 parts of high-activity polyether, 40-60 parts of slow-rebound polyether, 10-20 parts of PET recycled polyether, 0.1-0.4 part of a stabilizer, 0.4-1.0 part of a catalyst, 1-3 parts of a cross-linking agent, 0.4-0.8 part of a formaldehyde removal agent and 2-6 parts of a pore opening agent. The acoustic performance of the product obtained through the method is greatly improved, due to the fact that recycled materials and renewable materials are used, the carbon emission is reduced to a certain degree, the use effect is good, the production requirements of carpets with complex shapes and long pouring time can be met, the method is also compatible and applicable to carpets with simple structures, and the raw material compatibility is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane materials for automobile carpets, and in particular to a method for preparing a polyurethane foam material. Background Art

[0002] As an important component of automotive interior parts, the acoustic performance of polyurethane foam carpet directly affects the comfort of the driving environment. Therefore, it is urgent to develop a polyurethane soft foam formula with excellent acoustic performance. At the same time, low-carbon and environmentally friendly materials should be used in formula development to further improve the acoustic performance. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a method for preparing a polyurethane foam material. The prepared material has good acoustic performance and is environmentally friendly.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for preparing a polyurethane foam material, which is prepared from the following raw materials in parts by weight:

[0005] 40-60 parts of high-activity polyether, 40-60 parts of slow-rebound polyether, 10-20 parts of PET recycled polyether, 0.1-0.4 parts of stabilizer, 0.4-1.0 parts of catalyst, 1-3 parts of cross-linking agent, 0.4-0.8 parts of formaldehyde scavenger, and 2-6 parts of cell opener.

[0006] A preferred component is made of the following raw materials in parts by weight: 50 parts of high-activity polyether, 40 parts of slow-rebound polyether, 10 parts of recycled PET polyol, 0.3 parts of stabilizer, 0.4 parts of catalyst, 1 part of cross-linking agent, 0.4 parts of formaldehyde remover, and 4 parts of pore opener.

[0007] A preferred production method comprises the following steps:

[0008] The raw materials of high-activity polyether, slow-rebound polyether, PET recycled polyether, stabilizer, catalyst, cross-linking agent, formaldehyde scavenger and pore-opening agent are stirred at room temperature to obtain a combined polyether for use;

[0009] The slow-rebound MDI and the plant-based modified MDI were mixed in a ratio of 1:0.2 to obtain 72 parts of mixed MDI for later use;

[0010] Keep the combined polyether and mixed MDI at 15-25°C for later use;

[0011] The combined polyether and mixed MDI are mixed and injected into the mold through a high-pressure gun head with a pressure of 100-150 bar. The mold temperature is 60-80°C, the pressure holding time is 60-180s, and the mold is opened after molding to obtain the product.

[0012] Compared with the prior art, the present invention has the following beneficial effects: the acoustic performance of the product obtained by using the method is greatly improved, and the carbon emissions are reduced to a certain extent due to the use of recycled materials and renewable materials. The use effect is good, and the production requirements of carpets with complex shapes and long casting times can be met. It is also compatible with carpets with simple structures and good raw material compatibility. DETAILED DESCRIPTION

[0013] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0014] The present invention provides a method for preparing a polyurethane foam material, wherein the method develops a formula for the acoustic performance of polyurethane foam, improves the noise reduction performance of automobile carpets, and simultaneously reduces the carbon emissions of materials. The foam material prepared by the method is suitable for use as an environmentally friendly automobile carpet.

[0015] Embodiment 1:

[0016] The foaming material is made of the following components by weight: 50 parts of high-activity polyether, 40 parts of slow-rebound polyether, 10 parts of PET recycled polyether, 0.3 parts of stabilizer, 0.4 parts of catalyst, 1 part of cross-linking agent, 0.4 parts of formaldehyde remover, 4 parts of cell opener, and 72 parts of mixed MDI.

[0017] Production process:

[0018] (1) adding a high-activity polyether, a slow-rebound polyether, a PET-recovered polyether, a stabilizer, a catalyst, a cross-linking agent, a formaldehyde scavenger and a pore-opening agent to a stirring tank, and stirring at room temperature for 1 hour to obtain a combined polyether for use;

[0019] (2) adding the slow-rebound MDI and the plant-based modified MDI in a ratio of 1:0.2 into a stirring tank, stirring at room temperature for 1 hour to obtain a mixed MDI for use;

[0020] (3) The prepared combined polyether and mixed MDI are pumped into two material pre-storage tanks of the high-pressure foaming production line respectively, and the tank temperature is maintained at 15° C. for standby use;

[0021] (4) The combined polyether and mixed MDI in step (3) are mixed and injected into a mold through a high-pressure gun with a pressure of 100 bar. The mold temperature is 60° C. and the pressure holding time is 180 s. After molding, the mold is opened to obtain the product.

[0022] Embodiment 2:

[0023] The foaming material is made of the following components by weight: 40 parts of high-activity polyether, 60 parts of slow-rebound polyether, 20 parts of PET recycled polyether, 0.1 parts of stabilizer, 1 part of catalyst, 3 parts of cross-linking agent, 0.8 parts of formaldehyde remover, 2 parts of cell opener and 72 parts of mixed MDI.

[0024] Production process:

[0025] (1) adding a high-activity polyether, a slow-rebound polyether, a PET-recovered polyether, a stabilizer, a catalyst, a cross-linking agent, a formaldehyde scavenger and a pore-opening agent to a stirring tank, and stirring at room temperature for 1 hour to obtain a combined polyether for use;

[0026] (2) adding the slow-rebound MDI and the plant-based modified MDI in a ratio of 1:0.2 into a stirring tank, stirring at room temperature for 1 hour to obtain a mixed MDI for use;

[0027] (3) The prepared combined polyether and mixed MDI are pumped into two material pre-storage tanks of the high-pressure foaming production line respectively, and the tank temperature is maintained at 25° C. for standby use;

[0028] (4) The combined polyether and mixed MDI in step (3) are mixed and injected into a mold through a high-pressure gun with a pressure of 130 bar. The mold temperature is 70° C. and the pressure holding time is 150 s. After molding, the mold is opened to obtain the product.

[0029] Embodiment three:

[0030] The foaming material is made of the following components by weight: 60 parts of high-activity polyether, 50 parts of slow-rebound polyether, 15 parts of PET recycled polyether, 0.4 parts of stabilizer, 0.6 parts of catalyst, 1.5 parts of cross-linking agent, 0.6 parts of formaldehyde remover, 6 parts of cell opener, and 72 parts of mixed MDI.

[0031] Production process:

[0032] (1) adding a high-activity polyether, a slow-rebound polyether, a PET-recovered polyether, a stabilizer, a catalyst, a cross-linking agent, a formaldehyde scavenger and a pore-opening agent to a stirring tank, and stirring at room temperature for 1 hour to obtain a combined polyether for use;

[0033] (2) adding the slow rebound MDI and the plant-based modified MDI in a ratio of 1:0.2 into a stirring tank, stirring at room temperature for 1 hour to obtain the mixed MDI for use;

[0034] (3) The prepared combined polyether and mixed MDI are pumped into two material pre-storage tanks of the high-pressure foaming production line respectively, and the tank temperature is maintained at 20° C. for standby use;

[0035] (4) The combined polyether and mixed MDI in step (3) are mixed and injected into a mold through a high-pressure gun with a pressure of 150 bar. The mold temperature is 80° C. and the pressure holding time is 70 s. After molding, the mold is opened to obtain the product.

[0036] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a polyurethane foam material, characterized in that: Made from the following raw materials in parts by weight: 40-60 parts of high-activity polyether, 40-60 parts of slow-rebound polyether, 10-20 parts of PET recycled polyether, 0.1-0.4 parts of stabilizer, 0.4-1.0 parts of catalyst, 1-3 parts of cross-linking agent, 0.4-0.8 parts of formaldehyde scavenger, and 2-6 parts of cell opener.

2. The method for preparing the polyurethane foam material according to claim 1, characterized in that: Made from the following raw materials in parts by weight: 50 parts of high-activity polyether, 40 parts of slow-rebound polyether, 10 parts of recycled PET polyol, 0.3 parts of stabilizer, 0.4 parts of catalyst, 1 part of cross-linking agent, 0.4 parts of formaldehyde scavenger, and 4 parts of cell opener.

3. The method for preparing the polyurethane foam material according to claim 2, characterized in that: The method comprises the following steps: The raw materials of high-activity polyether, slow-rebound polyether, PET recycled polyether, stabilizer, catalyst, cross-linking agent, formaldehyde scavenger and pore-opening agent are stirred at room temperature to obtain a combined polyether for use; The slow rebound MDI and the plant-based modified MDI were mixed in a ratio of 1:0.2 to obtain 72 parts of mixed MDI for standby use; Keep the combined polyether and mixed MDI at 15-25°C for later use; The combined polyether and mixed MDI are mixed and injected into the mold through a high-pressure gun head with a pressure of 100-150 bar. The mold temperature is 60-80°C, the pressure holding time is 60-180s, and the mold is opened after molding to obtain the product.